Polyolefin film and preparation method thereof, battery separator and battery
By controlling the temperature-raising crystallinity and stretching ratio, the high-crystalline polyolefin raw materials and the three-step synergistic combination stretching strategy of low-ratio/high-ratio are used to prepare ultra-thin high-strength polyolefin films, which solves the thinning process of lithium-ion battery separators The problem of medium strength reduction improves battery performance and safety.
Patent Information
- Application Number
- CN202311193430.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-15
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-09-15
AI Technical Summary
The strength of the existing lithium-ion battery separator decreases during the thinning process, resulting in an increase in safety hazards. The multi-step synergistic high-speed stretching process is inefficient and easy to break the film, making it difficult to achieve the manufacturing of ultra-thin and high-strength separator.
By controlling the temperature-raising crystallinity and stretching ratio, a three-step synergistic stretching strategy of high-crystalline polyolefin raw materials and low-magnification/high-magnification three-step synergistic stretching strategy was used to prepare polyolefin films with a thickness of 1 to 5um, with a puncture strength of 300 to 1000gf. MD The tensile strength in the TD direction is ≥300MPa, the porosity is 25% to 45%, and the breathability is 20~80s/100cc.
Improve the crystallinity and orientation of the polyolefin substrate, reduce the risk of film breaking in the tensile step, improve production efficiency, and achieve ultra-thin, high puncture and high tensile strength in the battery separator, enhancing the battery Energy density and cycling performance reduce the safety risks brought about by mechanical failure.
Smart Images

Figure CN117352953B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of lithium ion batteries, and in particular to an ultra-thin high-strength polyolefin film and a preparation method thereof, a battery separator and a battery. Background Art
[0002] Lithium-ion batteries have the advantages of high operating voltage, high energy density, long cycle life, low self-discharge rate, low pollution, and no memory effect, and are widely used in new energy vehicles, new energy storage, consumer electronics and other fields. Further improving the energy density, cycle life and safety of lithium-ion batteries is a key research and development direction in the field of new energy. The diaphragm is one of the important components of lithium-ion batteries, which plays a role in blocking the electrolyte from the positive and negative electrodes. Because it is an inactive material in the battery, improving the energy density of the battery inevitably requires the diaphragm to be as thin as possible. However, the reduction in strength caused by the thinning of the diaphragm will further increase the safety risks during the use of the battery. Therefore, it is urgent to develop an ultra-thin and high-strength polyolefin diaphragm product.
[0003] At present, the conventional wet-process diaphragm manufacturing process mainly includes: high-temperature melting → die extrusion → casting → MD stretching → 1TD stretching → extraction → 2TD stretching → heat setting, or high-temperature melting → die extrusion → casting → simultaneous biaxial stretching → extraction → 2TD stretching → heat setting. Because the substrate is not fully stretched under this process, the thickness and strength of conventional diaphragm products are limited, which is not suitable for the manufacture of ultra-thin and high-strength diaphragm products.
[0004] Chinese invention patent CN109517210 A discloses an ultra-thin, high-strength polyolefin microporous membrane and its preparation method. Compared with the conventional wet diaphragm process, a stretching step is added after the extraction and drying steps to obtain a polyolefin microporous membrane with a thickness of 5 to 100 um, a puncture strength of more than 300 gf, and a tensile strength of more than 170 MPa; Chinese invention patent CN112592500B discloses a polyolefin porous membrane and its production system, battery diaphragm, and electrochemical device. Compared with the conventional wet diaphragm process, the temperature of the extractant is increased to obtain a polyolefin microporous membrane with a thickness of 2 to 30 um and a puncture strength of 1000 to 2000 gf; Chinese invention patent CN112290164 B discloses a high-performance additive suitable for producing ultra-thin lithium battery separators, and its preparation and application. By adding a low surface energy polymer, the surface energy of the melt is reduced, the lubricity of the melt during extrusion is improved, the plasticization and rheological properties of the melt are enhanced, and a polyethylene separator with a thickness of 3um is prepared; Chinese invention patent CN114204213 A discloses an ultra-thin polyolefin separator and its application. By screening polyethylene materials with specific molecular weight and melting characteristics, and controlling the extrusion amount, stretching temperature and stretching ratio during processing, an ultra-thin polyolefin separator with a thickness of ≤7um is obtained; Chinese invention patent CN114914631 A discloses an ultra-high strength separator and its preparation method. By adding a second longitudinal stretching + (second transverse stretching or synchronous biaxial stretching) before extraction, the stretching ratio is increased to obtain a thickness of 4-8um and a transverse tensile strength of 4000kgf / cm 2 , longitudinal tensile strength>4000kgf / cm 2 , a diaphragm with a needle puncture strength of ≥100gf / um; Chinese invention patent CN115020909 A discloses a diaphragm for lithium-ion batteries and a preparation method thereof, which is obtained by four biaxial / uniaxial stretching with a thickness of 3 to 8um and a tensile strength of >5000kgf / cm 2 , a lithium-ion battery separator with a needle puncture strength of >120gf / um; Chinese invention patent CN110815763 B discloses an apparatus and method for preparing a high-strength and high-modulus polyolefin film and a high-strength and high-modulus polyolefin film. By setting a cooling system and a multi-stage stretching machine, 10,000 times regional stretching is achieved to obtain a polyolefin film with a thickness of 2 to 100um, a tensile strength of 300 to 2000MPa, and a puncture strength of 50 to 300gf / um.
[0005] At present, the publicly available ultra-thin high-strength polyolefin separator manufacturing technology basically adopts a multi-step coordinated high-ratio stretching strategy, which easily leads to uneven force on the crystalline and non-crystalline regions of the polyolefin substrate during the high-ratio stretching process, resulting in frequent film breakage, reducing production efficiency, and thinning the separator often leads to lower puncture and tensile strength. Therefore, it is urgent to develop an efficient method for preparing ultra-thin high-strength polyolefin separators. Summary of the invention
[0006] The purpose of the present invention is to prepare an ultra-thin high-strength polyolefin film by controlling the crystallinity and stretching ratio during heating; and to use the film to make a battery separator, and to use the battery separator in a primary battery or a secondary battery, thereby improving the performance of the battery.
[0007] To achieve the above object, the present invention adopts the following technical solutions:
[0008] The invention provides a polyolefin film with a thickness of 1-5um, a puncture strength of 300-1000gf, a tensile strength in the MD direction of ≥300MPa, and a tensile strength in the TD direction of ≥300MPa.
[0009] Furthermore, the porosity of the polyolefin film is 25% to 45%, and the air permeability is 20 to 80s / 100cc.
[0010] Furthermore, the polyolefin film has a first-heating crystallinity of ≥80% and a second-heating crystallinity of ≥60% measured by a differential scanning calorimeter.
[0011] The present invention also provides a method for preparing a polyolefin film, which comprises the following steps:
[0012] (1) adding polyolefin, antioxidant and diluent into a screw extruder, melting into a uniform liquid at a temperature T1, extruding through a die head, and cooling at a temperature T2 to form a cast sheet;
[0013] (2) performing a first stretching on the cast sheet at a temperature of T3, and controlling the first stretching ratio to be 1 to 2.5 times, to obtain a first stretched film; the first stretching refers to sequentially performing a first longitudinal stretching (1MD) and a first transverse stretching (1TD), or performing a first biaxial synchronous stretching (1SBS);
[0014] (3) subjecting the once stretched film to a second stretching at a temperature of T4 to obtain a second stretched film; the second stretching refers to sequentially performing a second longitudinal stretching (2MD) and a second transverse stretching (2TD), or performing a second biaxial simultaneous stretching (2SBS);
[0015] (4) placing the secondary stretched film into an extraction tank at a temperature of T5 to completely elute the diluent, then placing the film into an oven at a temperature of T6 for drying, and then performing a third stretching at a temperature of T7 to obtain a tertiary stretched film; the third stretching refers to sequentially performing a third longitudinal stretching (3MD) and a third transverse stretching (3TD), or performing a third biaxial synchronous stretching (3SBS);
[0016] (5) The tertiary stretched film is heat-set at a temperature of T8 to obtain a polyolefin film.
[0017] Furthermore, the polyolefin includes but is not limited to one or more of polyethylene, polypropylene, polybutene, polypentene, ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-pentene copolymer, etc., which are synthesized by homopolymerization or copolymerization of olefin raw materials with carbon numbers of 2 to 10 in the molecules such as ethylene, propylene, butene, etc., and the total solid content is 10% to 60% of the total mass of the polyolefin and the diluent.
[0018] Furthermore, the polyolefin is preferably one or more of polyethylene, polypropylene, and ethylene-propylene copolymer, and the total solid content is 20% to 40% of the total mass of the polyolefin and the diluent.
[0019] Furthermore, the viscosity average molecular weight of the polyolefin is 350 to 2000 kDa.
[0020] Furthermore, the polyolefin has a first temperature rise crystallinity of ≥65% and a second temperature rise crystallinity of ≥45% as measured by a differential scanning calorimeter.
[0021] Furthermore, the antioxidant includes but is not limited to one or more of calcium stearate, magnesium stearate, zinc stearate, sodium stearate, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and n-octadecylβ-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.
[0022] Furthermore, the antioxidant is added in an amount of 0.01% to 1.0% of the mass of the polyolefin material.
[0023] Furthermore, the diluent includes but is not limited to one or more of white oil, paraffin oil, alkane compounds or ester compounds, which can be fully melt-mixed with polyolefin to form a uniform liquid at a temperature of the melting point of the polyolefin material + 50 to 100°C (i.e. 50 to 100°C higher than the melting point of the polyolefin material) without chemical reaction.
[0024] Furthermore, the extractant includes but is not limited to dichloromethane, carbon tetrachloride, ether and other solvents that are completely miscible with the diluent and are volatile.
[0025] Furthermore, the T1 temperature is the melting point of the polyolefin material + 50 to 100°C.
[0026] Furthermore, the T2 temperature is 5-30°C.
[0027] Furthermore, the T3 temperature is -10 to 40° C. above the melting point of the polyolefin material (ie, 10 to 40° C. lower than the melting point of the polyolefin material).
[0028] Furthermore, the T4 temperature is -10 to 40° C., which is the melting point of the polyolefin material.
[0029] Furthermore, the second stretching ratio is 7 to 15 times.
[0030] Furthermore, the T5 temperature is -10 to 30°C of the boiling point of the extractant.
[0031] Furthermore, the T6 temperature is the boiling point of the extractant + 0 to 20°C.
[0032] Furthermore, the T7 temperature is -10 to 40° C., which is the melting point of the polyolefin material.
[0033] Furthermore, the third stretching ratio is 3 to 7 times.
[0034] Furthermore, the T8 temperature is -40 to 60° C., which is the melting point of the polyolefin material.
[0035] The present invention also provides a battery separator, which comprises the polyolefin film.
[0036] Furthermore, the battery separator is a ceramic composite polyolefin separator or a polymer composite polyolefin separator coated on one or both sides of the polyolefin film.
[0037] Furthermore, the ceramic includes but is not limited to one or more of alumina, boehmite, lithium aluminum titanium phosphate, and silicon dioxide.
[0038] Furthermore, the polymer includes, but is not limited to, one or more of polyvinylidene fluoride, polymethyl methacrylate, aramid, polyimide, polyamide, polyoxazole, polysulfone, polyethersulfone, polyetheretherketone, and polyvinyl chloride.
[0039] Furthermore, the coating thickness is 0.2 to 1.5 um.
[0040] The present invention also provides a battery, comprising the battery separator as a component for separating positive and negative electrodes, and the battery is a primary battery or a secondary battery.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] (1) The innovation of the present invention lies in the selection of polyolefins with high crystallinity as the basic raw material, specifically, the selection of polyolefins with a crystallinity of ≥65% after the first heating and ≥45% after the second heating. Compared with polyolefins with low crystallinity, the present invention can improve the crystallinity and orientation of the molecular chain segments of the polyolefin substrate in each process stage, increase the force consistency between the crystalline region and the amorphous region of the polyolefin substrate during the stretching process, further improve the stretchability of the polyolefin substrate, reduce the risk of film breakage in the stretching step, and improve production efficiency.
[0043] (2) The innovation of the present invention also lies in the strategy of adopting a low-ratio stretching in the first stretching process, specifically, a 1-2.5-ratio stretching. Compared with a high-ratio stretching (more than 3 times), this can more effectively improve the crystallinity of the polyolefin substrate and the orientation of the polyolefin molecular chain forging, thereby providing a guarantee for the second and third high-ratio stretching steps, reducing the risk of film breakage during the second and third high-ratio stretching processes, and improving production efficiency.
[0044] (3) The innovation of the present invention also lies in the use of a high-crystallinity polyolefin raw material and a low-ratio / high-ratio three-step synergistic combined stretching strategy. By selecting a high-crystallinity polyolefin raw material and adopting the first low-ratio stretching, an environment that is beneficial to improving the crystallinity and orientation is maintained on the basis of the original high crystallinity. Through this synergistic effect, the crystallinity and orientation are further improved, and a high-crystallinity polyolefin film with a first-heating crystallinity of ≥80% and a second-heating crystallinity of ≥60% is obtained, and its thickness is controlled to be 1-5um. After testing, its puncture strength is 300-1000gf, the tensile strength in the MD direction is ≥300MPa, and the tensile strength in the TD direction is ≥300MPa, which has the characteristics of ultra-thinness, high puncture strength and high tensile strength.
[0045] (4) The prepared polyolefin film is made into a battery separator and applied to primary or secondary batteries, which can effectively increase the capacity of battery active materials, reduce battery internal resistance, improve the energy density and cycle performance of secondary batteries, and effectively reduce the safety risks caused by mechanical failure of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is a scanning electron microscope photograph of the surface of Example 1.
[0047] Figure 2 This is a scanning electron microscope photograph of the surface of Comparative Example 1. DETAILED DESCRIPTION
[0048] In order to make the various technical features and advantages or technical effects in the above technical solutions of the present invention more obvious and easy to understand, they are described in detail below with reference to the accompanying drawings.
[0049] Example 1
[0050] As shown in the physical property parameters in Table 1, polyethylene, calcium stearate and white oil were added into the screw extruder, and dichloromethane was used as the extractant. Under the process parameters in Table 2, an ultra-thin high-strength polyolefin film was obtained, and its properties were shown in Table 3.
[0051] Example 2
[0052] As shown in the physical property parameters in Table 1, polyethylene, calcium stearate and white oil were added into the screw extruder, and dichloromethane was used as the extractant. Under the process parameters in Table 2, an ultra-thin high-strength polyolefin film was obtained, and its properties were shown in Table 3.
[0053] Example 3
[0054] As shown in the physical property parameters in Table 1, polyethylene, calcium stearate and white oil were added into the screw extruder, and dichloromethane was used as the extractant. Under the process parameters in Table 2, an ultra-thin high-strength polyolefin film was obtained, and its properties were shown in Table 3.
[0055] Example 4: As shown in Table 1, polyethylene, calcium stearate and white oil are added into a screw extruder, and dichloromethane is used as an extractant. Under the process parameters in Table 2, an ultra-thin high-strength polyolefin film is obtained, and its properties are shown in Table 3.
[0056] Example 5
[0057] As shown in Table 1, polyethylene, calcium stearate and white oil were added into a screw extruder, and dichloromethane was used as an extractant. Film samples were obtained under the process parameters in Table 2, and their properties are shown in Table 3.
[0058] Comparative Example 1
[0059] As shown in the physical property parameters in Table 1, polyethylene, calcium stearate and white oil were added into the screw extruder, and dichloromethane was used as the extractant. Under the process parameters in Table 2, an ultra-thin high-strength polyolefin film was obtained, and its properties were shown in Table 3.
[0060] In the above embodiment, the melting point of polyethylene is 137°C, and the boiling point of dichloromethane is 40°C.
[0061] In the above embodiment, a differential scanning calorimeter (DSC) is used to test the crystallinity of polyolefin materials and films. Under 25°C, the sample is heated to 40°C above the melting point of the material for the first time at 10°C / min to obtain the first heating crystallinity, then cooled to below 25°C at 10°C / min, and then heated to 40°C above the melting point of the material for the second time at 10°C / min to obtain the second heating crystallinity. Specifically, the first heating crystallinity of polyolefin is obtained by dividing the melting enthalpy of polyolefin measured during the first heating process by the standard melting enthalpy of polyolefin. Among them, the standard melting enthalpy of polyethylene is 293J / g.
[0062] In the above embodiment, the thickness, air permeability, porosity, puncture strength and tensile strength of the polyolefin film are tested according to GB / T 36363-2018.
[0063] In the above embodiment, the film samples are assembled into LFP / / diaphragm / / Li batteries, and the charge and discharge experiments are carried out at room temperature 0.1C and between 2.5 and 4.0V to test the discharge specific capacity and the capacity retention rate after 100 cycles at room temperature 1C. The lithium iron phosphate (LFP) positive electrode is composed of 80wt% LiFePO4, 10wt% PVDF and 10wt% carbon black.
[0064] Table 1 Physical properties and proportions of raw materials in the embodiment
[0065]
[0066] Table 2 Process parameters of the implementation method
[0067]
[0068] Table 3 Performance of the implementation method
[0069]
[0070] like Figure 1 As shown, the ultra-thin high-strength film (Example 1) prepared by the present invention has a uniform distribution of fiber diameters on its surface and abundant pores due to the use of high-crystallinity polyolefin raw materials and a low-rate / high-rate three-step synergistic combination stretching strategy, indicating that the polyethylene molecular chains are subjected to uniform force during the stretching process and the substrate is fully stretched in all directions. Figure 2 The surface SEM image of the polyethylene film (Comparative Example 1) prepared using a low-crystallinity polyolefin raw material and a two-step high-ratio stretching strategy shows that the surface pores are relatively small and unevenly distributed, indicating that the polyolefin substrate cannot be fully stretched under this strategy.
[0071] As shown in Table 3, Example 1 uses polyethylene with a first heating crystallinity of 68.7% and a second heating crystallinity of 57.1% as a raw material, and obtains a film sample with a thickness of 5 microns, a puncture strength of 1000gf, an MD tensile strength of 410MPa, and a TD tensile strength of 435MPa through a three-step small-rate + large-rate synergistic stretching process of 1.5*1.5+10*10+5*5. The film sample is applied to a secondary battery with LFP as the positive electrode, and the discharge specific capacity is 152.1mAh / g. The capacity after 100 cycles is The retention rate is 83.6%; while Comparative Example 1 uses polyethylene with a crystallinity of 45.3% in the first heating and 27.1% in the second heating as raw materials, and obtains a film sample with a thickness of 5 microns, a puncture strength of 435gf, a MD tensile strength of 198MPa, and a TD tensile strength of 215MPa through a two-step high-ratio stretching process of 10*10+5*5. It is applied to a secondary battery with LFP as the positive electrode, and the discharge specific capacity is 151.2mAh / g, and the capacity retention rate after 100 cycles is 80.1%. It can be seen from the data of Example 1 and Comparative Example 1 above that the use of high-crystallinity raw materials combined with a three-step coordinated stretching process can significantly improve the strength of polyethylene film and battery performance.
[0072] As shown in Table 3, Example 5 uses polyethylene with a first heating crystallinity of 65.2% and a second heating crystallinity of 45.6% as a raw material, and obtains a film sample with a thickness of 1 micron, a puncture strength of 310gf, an MD tensile strength of 311MPa, and a TD tensile strength of 315MPa through a three-step small-rate + large-rate synergistic stretching process of 2*2+15*15+3*3. The film sample is applied to a secondary battery with LFP as the positive electrode, and the discharge specific capacity is 153.6mAh / g, and the capacity retention rate after 100 cycles is 84.7%. Compared with Comparative Example 1, the capacity is increased by 2.4mAh / g, and the cycle capacity retention rate is increased by 4.6%.
[0073] In the embodiments of the present invention, a polyolefin film with ultra-thin and high-strength characteristics is obtained by selecting high-crystallinity raw materials and combining a synergistic combined stretching process, which can be applied to secondary batteries to significantly improve battery performance.
[0074] Although the present invention has been disclosed as above by way of embodiments, it is not intended to limit the present invention. Appropriate modifications or equivalent substitutions of the technical solutions of the present invention made by ordinary technicians in the field should all be included in the protection scope of the present invention. The protection scope of the present invention shall be based on what is defined in the claims.
Claims
1. A method for preparing a polyolefin film, characterized in that: The following steps are involved: (1) adding polyolefin, antioxidant and diluent into a screw extruder, melting into a uniform liquid at a temperature T1, extruding through a die head, cooling at a temperature T2, and forming a casting sheet; the temperature T1 is the melting point of the polyolefin material minus 50 to 100° C., and the temperature T2 is 5 to 30° C.; (2) performing a first stretching on the cast sheet at a temperature of T3, and controlling the ratio of the first stretching to be 1 to 2.5 times, to obtain a first stretched film; the first stretching refers to sequentially performing a first longitudinal stretching and a first transverse stretching, or performing a first biaxial simultaneous stretching; the temperature of T3 is the melting point of the polyolefin material minus 10 to 40° C.; (3) subjecting the once stretched film to a second stretching at a temperature of T4, wherein the second stretching ratio is 7 to 15 times, to obtain a second stretched film; the second stretching refers to sequentially conducting a second longitudinal stretching and a second transverse stretching, or conducting a second biaxial simultaneous stretching; the T4 temperature is the melting point of the polyolefin material minus 10 to 40°C; (4) placing the secondary stretched film into an extraction tank at a temperature of T5 to completely elute the diluent, then placing the film into an oven at a temperature of T6 for drying, and then performing a third stretching at a temperature of T7, wherein the third stretching ratio is 3 to 7 times, to obtain a tertiary stretched film; the third stretching refers to sequentially performing a third longitudinal stretching and a third transverse stretching, or performing a third biaxial simultaneous stretching; the temperature of T5 is the boiling point of the extractant minus 10 to 30° C., the temperature of T6 is the boiling point of the extractant plus 0 to 20° C., and the temperature of T7 is the melting point of the polyolefin material minus 10 to 40° C.; (5) heat setting the tertiary stretched film at a temperature of T8 to obtain a polyolefin film; the T8 temperature is the melting point of the polyolefin material minus 40 to 60°C.
2. The method according to claim 1, characterized in that The polyolefin is one or more of polyethylene, polypropylene, polybutene, polypentene, ethylene-propylene copolymer, ethylene-butene copolymer, and ethylene-pentene copolymer synthesized from olefin raw materials with carbon numbers of 2 to 10 by homopolymerization or copolymerization, and the total solid content is 20% to 40% of the total mass of the polyolefin and the diluent; the viscosity-average molecular weight of the polyolefin is 350 to 2000 kDa.
3. The method according to claim 1, characterized in that The polyolefin has a first-heating crystallinity of ≥65% and a second-heating crystallinity of ≥45% measured by a differential scanning calorimeter.
4. The method according to claim 1, characterized in that The antioxidant is one or more of calcium stearate, magnesium stearate, zinc stearate, sodium stearate, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and n-octadecylβ-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate; the antioxidant is added in an amount of 0.01% to 1.0% of the mass of the polyolefin; The diluent is one or more of white oil, paraffin oil, alkane compounds, and ester compounds, which can be fully melted and mixed with the polyolefin to form a uniform liquid at a temperature of 50 to 100° C. above the melting point of the polyolefin material without chemical reaction; The extractant is one of dichloromethane, carbon tetrachloride and ether.
5. The method according to claim 1, characterized in that The prepared polyolefin film has a thickness of 1 to 5 μm, a puncture strength of 300 to 1000 gf, a tensile strength in the MD direction of ≥300 MPa, a tensile strength in the TD direction of ≥300 MPa, a porosity of 25% to 45%, and an air permeability of 20 to 80 s / 100 cc; the first-temperature crystallinity measured by a differential scanning calorimeter is ≥80%, and the second-temperature crystallinity is ≥60%.
6. A battery separator, characterized in that: A composite polyolefin diaphragm prepared by coating ceramic or polymer powder on one or both sides of a polyolefin film prepared by the method described in any one of claims 1 to 5; The ceramic is one or more of alumina, boehmite, lithium aluminum titanium phosphate, and silicon dioxide; The polymer is one or more of polyvinylidene fluoride, polymethyl methacrylate, aramid, polyimide, polyamide, polyoxazole, polysulfone, polyethersulfone, polyetheretherketone, and polyvinyl chloride; The coating thickness is 0.2~1.5um.
7. A battery, characterized in that: The battery comprises the battery separator according to claim 6 as an element for separating positive and negative electrodes, and the battery is a primary battery or a secondary battery.
Citation Information
Patent Citations
Ultrathin high strength polyolefin microporous membrane and preparation method thereof
CN109517210A
Equipment and methods for preparing high-strength, high-modulus polyolefin films and high-strength, high-modulus polyolefin films
CN110815763B
A high-performance additive suitable for the production of ultra-thin lithium battery separators, its preparation and application
CN112290164B
A polyolefin microporous membrane and its production system, a battery separator, and an electrochemical device.
CN112592500B
Ultrathin polyolefin membranes and uses
CN114204213A