Bamboo fluff pulp board and preparation method
Through multiple screening treatments and the addition of debonding agents, the bamboo fiber length distribution is adjusted to form a bamboo fluff pulp board with excellent fluff and water absorption properties, which solves the problems of bamboo fluff pulp performance differences and fiber waste in the existing technology, and achieves Efficient fiber utilization and performance improvements.
Patent Information
- Application Number
- CN202311302484.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-08
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-10-08
AI Technical Summary
The existing bamboo fluff pulp preparation method cannot meet the comprehensive utilization of fiber in the screening process, resulting in large differences in performance of bamboo fluff pulp prepared from different bamboo materials, serious fiber waste, and difficulty in achieving good fluff and absorption properties.
The length distribution of bamboo fibers is adjusted through multiple screening processes so that the proportion of fibers <0.4mm is less than 1%, the proportion of fibers 0.4-0.85mm is 4-6.5%, and the proportion of fibers ≥1.7mm is greater than or equal to 60% , and add a debonding agent to the fibers to form a bamboo fluff pulp board with a kink fiber ratio of 57-66%.
The complete raising and fluffing time of bamboo fluff pulp board is less than 40 seconds, the tightness is 0.5-0.6g/cm3, the dry bulk is greater than 25cm3/g, the water absorption is greater than 9g/g, and the fiber utilization rate is improved, and the performance is close to that of softwood fluff pulp. , adapted to the use of different bamboo materials.
Smart Images

Figure BDA0004487819760000061 
Figure BDA0004487819760000071
Abstract
Description
Technical Field
[0001] The present application relates to pulp, and in particular to a bamboo fluff pulp board and a preparation method thereof. Background Art
[0002] In recent years, the global demand for fluff pulp has been growing at an annual rate of 5%. my country's annual demand for fluff pulp has reached millions of tons. However, fluff pulp still mainly relies on wood fiber, especially coniferous wood fiber. Research has found that bamboo pulp fiber is close to coniferous pulp in terms of cushion thickness and other aspects, making it the most convenient means and possibility to convert bamboo pulp fiber into fluff pulp fiber. By preparing bamboo fluff pulp, the bamboo pulp industry is promoted to enter higher value-added application areas.
[0003] At present, some institutions have studied and applied bamboo pulp for the preparation of fluff pulp. In order to meet the performance requirements of fluff pulp in terms of napping, fluffiness, water absorption, etc., the pulp is usually pre-treated by screening treatment. More specifically, it is necessary to remove the miscellaneous cells and fine fibers in the bamboo pulp by screening treatment during the pulping or papermaking process. For example, the document number CN114687234A, entitled: A method for preparing fluff pulp using bamboo and the method recorded in the patent document of the prepared fluff pulp, and the document number CN114855496A, entitled: A method for preparing bamboo fluff pulp and a method recorded in the patent document of the product thereof, but these methods still have the following problems:
[0004] First, in order to achieve comprehensive utilization of fibers, usually in the screening process, only fibers below 0.5 mm or even 0.3 mm are screened and removed, but the bamboo fluff pulp prepared after such treatment still cannot meet the actual needs;
[0005] 2. Due to the large difference in fiber distribution among different types of bamboo, the following table lists the approximate distribution of fiber length among different types of bamboo:
[0006] Types of Bamboo 0-1.0mm 1.0-1.5mm 1.5-2mm 2.0-2.5mm 2.5-3.0mm 3.0mm or more Green Bamboo 10 19.4 30.4 21.9 10.2 8.1 Green bamboo 4 12.7 21 22.4 17.7 22.2 big wood bamboo 5 13.5 21.9 23 17.1 19.5 Bamboo 11 18 23 21 17 10 bamboo 6.5 18.5 28 22 15.5 9.5
[0007] Due to the huge difference in fiber distribution, the properties of bamboo fluff pulp prepared from different bamboos vary greatly;
[0008] 3. In order to achieve better raising and absorption performance, CN114855496A further uses only fibers with a diameter of 1.65-1.90 mm to prepare fluff pulp, but this method will cause a huge waste of fibers.
[0009] Therefore, a fluff pulp board is needed that has good performance while being adaptable to different bamboo species. Summary of the invention
[0010] The present application provides a bamboo fluff pulp board, which has a complete fluffing and decomposition time of less than 40 seconds and a density of 0.5-0.6 g / cm 3 , dry bulk greater than 25cm 3 / g, the water absorption is greater than 9g / g, and the bamboo fluff pulp board includes bamboo fibers, and the bamboo fibers have the following distribution according to length:
[0011] Bamboo fibers smaller than 0.4 mm account for less than 1%;
[0012] 0.4-0.85mm bamboo fiber 4-6.5%;
[0013] Bamboo fiber ≥1.7mm accounts for 60% or more;
[0014] Moreover, the proportion of kinked fibers is 57-66%.
[0015] The average length of the bamboo fibers is greater than or equal to 1.6 mm, and the proportion of broken fibers is less than or equal to 12%.
[0016] Wherein, the fibers in the bamboo fluff pulp board are all bamboo fibers.
[0017] Among them, the bamboo fiber with a diameter of 0.4-0.85 mm accounts for 5.8-6.5%, and the complete fluffing and decomposition time is less than 35 seconds.
[0018] The present invention also provides a method for preparing the above-mentioned bamboo fluff pulp board, comprising the following steps:
[0019] S1: providing initial bamboo pulp;
[0020] S2: adjusting the fiber distribution of the initial bamboo pulp to obtain the bamboo pulp to be used, wherein the bamboo fibers of less than 0.4 mm account for less than 1%; the bamboo fibers of 0.4-0.85 mm account for 4-6.5%; and the bamboo fibers of ≥1.7 mm account for greater than or equal to 60%;
[0021] S3: The bamboo pulp to be used is papermade to obtain a bamboo fluff pulp board.
[0022] Wherein, step S2 is formed in the following manner:
[0023] S21: performing a first screening process on the initial bamboo pulp to obtain a first bamboo pulp having a fiber length greater than 0.85 mm and a second bamboo pulp having a fiber length less than 0.85 mm;
[0024] S22: performing a second screening process on the first bamboo pulp to obtain a third bamboo pulp having a fiber length of greater than or equal to 1.7 mm and a fourth bamboo pulp having a fiber length of 0.85-1.7 mm, and performing a third screening process on the second bamboo pulp to obtain a fifth bamboo pulp having a fiber length of 0.4-0.85 mm;
[0025] S23: adding the third bamboo pulp and the fifth bamboo pulp to the fourth bamboo pulp to form standby bamboo pulp, wherein the proportion of bamboo fibers with a diameter of 0.4-0.85 mm in the standby bamboo pulp is 4-6.5%, and the proportion of bamboo fibers with a diameter of 1.7 mm or larger is greater than or equal to 60%.
[0026] Among them, after the second screening process and the third screening process, the third bamboo pulp and the fifth bamboo pulp are transported to the corresponding storage tanks, and then the third bamboo pulp and the fifth bamboo pulp in the corresponding storage tanks are transported to the pulp mixing system, and the pulp mixing system mixes the fourth bamboo pulp, the third bamboo pulp and the fifth bamboo pulp to form the stand-by bamboo pulp.
[0027] Wherein, in step S23, the proportion of bamboo fibers with a diameter of 0.4-0.85 mm in the bamboo pulp to be used is 5.8-6.5%.
[0028] Beneficial effect: A bamboo fluff pulp board, the complete fluffing time is less than 40s, and the density is 0.5-0.6g / cm 3 , dry bulk greater than 25cm 3 / g, water absorption is greater than 9g / g, and the bamboo fluff pulp board includes bamboo fibers, and the bamboo fibers have the following distribution according to length: bamboo fibers <0.4mm account for less than 1%; bamboo fibers 0.4-0.85mm account for 4-6.5%; bamboo fibers ≥1.7mm account for greater than or equal to 60%; and twisted fibers account for 57-66%. By adjusting the fiber distribution in the bamboo fluff pulp, the prepared bamboo fluff pulp board has an absorption performance close to that of coniferous wood fluff pulp and obtains good raising performance. On the other hand, different types of bamboo materials can obtain basically consistent performance. The present invention also provides a preparation method for the above-mentioned bamboo fluff pulp board. DETAILED DESCRIPTION
[0029] The present application is further described in detail below in conjunction with the embodiments. It is particularly noted that the following embodiments are only used to illustrate the present application, but are not intended to limit the scope of the present application. Similarly, the following embodiments are only partial embodiments of the present application rather than all embodiments, and all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present application.
[0030] The present invention provides a bamboo fluff pulp board, which has good fluffing performance. More specifically, the fluff pulp board has a complete fluffing time of less than 40 seconds and a tightness of 0.5-0.6 g / cm 3 , dry bulk greater than 24cm 3 / g, and the water absorption is greater than 9g / g, which can meet the technical indicators of coniferous wood fluff pulp.
[0031] It can be understood that the bamboo fluff pulp board includes bamboo fibers. More specifically, the bamboo fluff pulp board is a plate-like or sheet-like material formed by papermaking of bamboo fibers. It can be understood that the bamboo fluff pulp board can be stacked in a roll or sheet shape. When the bamboo fluff pulp board is in a roll shape, it has a longer extension along the MD direction and is wound into a cylindrical shape.
[0032] In the present invention, the bamboo fiber content in the bamboo fluff pulp board is greater than or equal to 92%. More specifically, the bamboo fluff pulp board does not contain other plant fibers, such as wood pulp fibers, straw pulp fibers, etc., that is, 100% of the fibers in the bamboo fluff pulp board are bamboo fibers.
[0033] In the present invention, the bamboo fibers have the following distribution according to length:
[0034] Bamboo fibers smaller than 0.4 mm account for less than 1%;
[0035] 0.4-0.85mm bamboo fiber accounts for 4-6.5%;
[0036] The proportion of bamboo fiber ≥1.7mm is greater than or equal to 60%.
[0037] At the same time, when the proportion of twisted fibers is 57-66%, the prepared bamboo fluff pulp board has performance close to that of coniferous wood fluff pulp or is basically equivalent to that of coniferous wood fluff pulp.
[0038] Preferably, the proportion of bamboo fibers with a diameter of 0.4-0.85 mm is 5.8-6.5%. In this case, the time required for the fluff pulp board to be completely fluffed can be less than 35 seconds.
[0039] The above-mentioned bamboo fiber proportions are all calculated by quantity.
[0040] The applicant found in the research:
[0041] First, for fluff pulp, absorption performance is one of its most important properties, especially when used to prepare the core of absorbent products, longer fibers can have better absorption performance. Therefore, people in the field believe that longer fibers should be used to prepare fluff pulp. This is also the reason why coniferous wood fiber is used as the main raw material for fluff pulp in the field. However, the applicant found in the study that since the aspect ratio of bamboo fiber is larger than that of coniferous wood fiber, bamboo fiber is more slender than wood fiber. More specifically, the aspect ratio of coniferous wood fiber is approximately 60-80, such as the average aspect ratio of Masson pine is 72, the average aspect ratio of Korean pine is 67, and the average aspect ratio of larch is 77, while the aspect ratio of bamboo fiber is greater than 100, such as the average aspect ratio of Phyllostachys chinensis is 111, and the average aspect ratio of Phyllostachys viridiflora is 139. In this case, on the one hand, bamboo fiber is more likely to have fiber kinks and entanglements than coniferous wood fiber, making it difficult to raise the bamboo fiber. On the other hand, the formed pulp board is denser, which will also make it difficult to raise the bamboo fiber pulp board.
[0042] 2. The study found that when a certain amount of short bamboo fibers are appropriately added to bamboo fibers or relatively short bamboo fibers are in a suitable proportion, these short bamboo fibers will be dispersed and filled between long fibers. On the one hand, the proportion of kinks in bamboo fibers will be reduced, thereby improving the raising performance. On the other hand, the compactness of the pulp board can be reduced, thereby improving the raising properties of bamboo fibers.
[0043] 3. At the same time, it was found that short bamboo fibers should be in an appropriate proportion. That is, when the proportion of short fibers is too high, on the one hand, the absorption performance is reduced, and the amount of dust in the subsequent crushing and defibration process is too large, causing inconvenience in subsequent production. In further research, it was found that the appropriate length of short fibers is 0.4-0.85mm, and the appropriate proportion of this part is 4-6.5%.
[0044] Fourth, by adjusting the fiber distribution and making the fibers of 0.4-0.85mm and larger than 1.7mm in an appropriate proportion, the proportion of entangled fibers is also in an appropriate range, specifically 57-66% of entangled fibers, so that the formed bamboo fluff pulp has good raising properties while other properties such as fluffiness and tightness can approach or reach the level of wood fibers.
[0045] Furthermore, the average length of the bamboo fibers is greater than or equal to 1.6 mm, so that the bamboo fluff pulp has better absorption performance, and the core prepared by using the bamboo fluff pulp board has better absorption performance.
[0046] Furthermore, the broken fiber ratio of the bamboo fiber should be less than or equal to 12%.
[0047] Furthermore, the quantitative deviation of the pulp board does not exceed ±5%, so that the pulp board has good and uniform fiber distribution. During the pulp board raising process, the fiber peeling strength from the pulp board is basically consistent, thereby producing a uniform single fiber effect without the phenomenon of clumps of fibers being separated from the pulp board.
[0048] In order to further illustrate the present invention, the preparation of the bamboo fluff pulp will be described below:
[0049] S1: providing initial bamboo pulp.
[0050] The initial bamboo pulp can be a fiber raw material made from bamboo materials such as moso bamboo, nan bamboo, citron bamboo, big wood bamboo, and large-leaf dragon bamboo through pulping methods such as sulfate method or caustic soda method. At the same time, the initial bamboo pulp can be natural bamboo pulp or bleached bamboo pulp. The fiber length of the initial bamboo pulp is 0.2-6 mm. At the same time, the initial bamboo pulp can be a mixture of one or more of the above-mentioned fiber raw materials. The concentration of the initial bamboo pulp is 0.5%-6%. The initial bamboo pulp can be stored in a pulp storage tank for subsequent use.
[0051] It can be understood that the preliminary bamboo pulp can be prepared by the method given in CN113249999A, etc.
[0052] S2: The fiber distribution of the initial bamboo pulp is adjusted to obtain the ready-to-use bamboo pulp, wherein: the bamboo fibers with a diameter less than 0.4 mm account for less than 1%; the bamboo fibers with a diameter between 0.4 and 0.85 mm account for 4 to 6.5%; and the bamboo fibers with a diameter greater than or equal to 1.7 mm account for greater than or equal to 60%.
[0053] Specifically, adjustments are made in the following ways:
[0054] S21: Performing a first screening process on the initial bamboo pulp to obtain a first bamboo pulp with a fiber length greater than 0.85 mm and a second bamboo pulp with a fiber length less than 0.85 mm.
[0055] Specifically, a screening device can be used for screening treatment, the screening device includes a containing space and a screen, the screen divides the containing space into a first channel and a second channel, the screen is provided with a plurality of screen holes, relatively short fibers can pass through the screen and then be discharged through the second channel, and relatively long fibers can be transported through the first channel. In a specific embodiment, a screening device as shown in CN114481666A or CN113622212A can be used for screening treatment;
[0056] S22: The first bamboo pulp is subjected to a second screening process to obtain a third bamboo pulp having a fiber length greater than or equal to 1.7 mm and a fourth bamboo pulp having a fiber length of 0.85-1.7 mm, and the second bamboo pulp is subjected to a third screening process to obtain a fifth bamboo pulp having a fiber length of 0.4-0.85 mm.
[0057] Similarly, the screening process is performed by a screening device. It can be understood that the sieve hole diameter of the screening device used in the second screening process and the sieve hole diameter of the screening device used in the third screening process are different from the sieve hole diameter of the screening device used in the first screening process.
[0058] S23: adding the third bamboo pulp and the fifth bamboo pulp to the fourth bamboo pulp to form standby bamboo pulp, wherein the proportion of bamboo fibers with a diameter of 0.4-0.85 mm in the standby bamboo pulp is 4-6.5%, and the proportion of bamboo fibers with a diameter of 1.7 mm or larger is greater than or equal to 60%.
[0059] It is understandable that before performing step S23, the concentrations of the fourth bamboo pulp, the third bamboo pulp and the fifth bamboo pulp may be tested first, and the required amount of each bamboo pulp may be proportioned according to the concentration of each bamboo pulp.
[0060] It can be understood that after the second screening process, the third bamboo pulp and the fifth bamboo pulp are transported to the corresponding storage tanks, and then the third bamboo pulp and the fifth bamboo pulp in the corresponding storage tanks are transported to the pulp mixing system, and the pulp mixing system mixes the fourth bamboo pulp, the third bamboo pulp and the fifth bamboo pulp to form the stand-by bamboo pulp.
[0061] In this way, the initial bamboo pulp formed by different raw materials can finally form the standby bamboo pulp with basically the same fiber distribution. For example, when using bamboo with higher short fiber content and bamboo with lower short fiber content, standby bamboo pulp with basically the same performance can be obtained.
[0062] It is understandable that the bamboo fibers with a length less than 0.4 mm in the bamboo pulp to be used should be less than 1%.
[0063] Preferably, the bamboo fibers with a diameter of 0.4-0.85 mm account for 5.8-6.5% of the bamboo pulp to be used.
[0064] Furthermore, before step S23, the step of adding a debonding agent to the fifth bamboo pulp is also included. This is because the fifth bamboo pulp is a relatively short bamboo fiber with a larger specific surface area. On the one hand, it can better absorb the debonding agent. On the other hand, after adsorbing the debonding agent, it can be more and more evenly dispersed among longer fibers, thereby reducing the bonding force between the fibers and achieving a better raising effect.
[0065] Furthermore, the dosage of the debonding agent is 0.1%-0.6%.
[0066] S3: The bamboo pulp to be used is papermade to obtain a bamboo fluff pulp board.
[0067] It is understandable that the concentration of the bamboo pulp to be used can also be adjusted / diluted by the recovered clean water to obtain a suitable bamboo pulp concentration for papermaking, and then papermaking is performed to obtain the fluff pulp board.
[0068] The present invention will be further described below in conjunction with specific embodiments:
[0069] Example 1: The bamboo fluff pulp board obtained by the above preparation method has the following fiber length distribution: <0.4 mm accounts for 0.9%; 0.4-0.85 mm accounts for 6.1%; 0.85-1.7 mm accounts for 31.2%; ≥1.7 mm accounts for 61.9%; and twisted fibers account for 63.2%.
[0070] Example 2: The bamboo fluff pulp board obtained by the above preparation method, <0.4mm accounts for 0.4%; 0.4-0.85mm accounts for 4.1%; 0.85-1.7mm accounts for 26.3%; ≥1.7mm accounts for 69.2%; twisted fibers account for 59.2%.
[0071] Example 3: The bamboo fluff pulp board obtained by the above preparation method, <0.4mm accounts for 0.8%; 0.4-0.85mm accounts for 6.4%; 0.85-1.7mm accounts for 28.1%; ≥1.7mm accounts for 64.6%; twisted fibers account for 60.9%.
[0072] Comparative Example 1: The classification treatment method of CN114481666A is adopted to obtain bamboo fluff pulp with a diameter of 1.7 mm or more, in which fibers with a diameter of 1.7 mm or more account for 99% or more of the fiber distribution.
[0073] Comparative Example 2: The grading treatment method of CN114481666A is adopted to obtain bamboo fluff pulp with a diameter of 0.4-1.7 mm, in which the proportion of fibers with a diameter of 0.4-1.7 mm in the fiber distribution is greater than or equal to 98%.
[0074] Comparative Example 3: The grading treatment method of CN114481666A is adopted to only grade the bamboo pulp fibers (i.e., only bamboo fibers below 0.4 mm are screened out, and the fiber distribution is not adjusted), but the fibers with a length of 0.4-0.85 mm account for 3.5%, and the fiber raw material is large bamboo.
[0075] Comparative Example 4: The classification treatment method of CN114481666A is adopted, and only the bamboo pulp fibers are classified (i.e., only the bamboo fibers below 0.4 mm are screened out, and the fiber distribution is not adjusted), but the fibers with a length of 0.4-0.85 mm account for 7.5%, and the fibers with a length greater than 1.7 mm account for 59%, and the raw material is green bamboo;
[0076] Comparative Example 5: The initial bamboo pulp is not subjected to classification treatment, and the fluff pulp board is directly prepared.
[0077] Comparative Example 6: The processing method of Example 1 of CN114855496A is adopted, and the proportion of fibers with a diameter of 1.65-1.9 mm is greater than 99%;
[0078] Comparative Example 7: Existing softwood fluff pulp 1;
[0079] Comparative Example 8: Existing softwood fluff pulp 2;
[0080] The above examples and comparative examples were tested for physical properties, and the results were as follows:
[0081]
[0082]
[0083] In the above tests, the testing standards / methods for the relevant physical property indicators are as follows:
[0084] Quantitative test: Samples are taken according to GB / T740, and the sample processing and test standard atmosphere are carried out according to GB / T10739; the treated sample is weighed and divided by the sample area 0.0314m2 to obtain the fluff pulp quantity.
[0085] Tightness test: According to GB / T451.3, after measuring the thickness of the sample, divide the quantitative value by the thickness.
[0086] Bursting index test: According to GB / T1539, use a cardboard bursting tester to measure ten groups of data on the front and back of the fluff pulp board, calculate the average value, and then divide it by the quantitative value to get the bursting index.
[0087] Determination of dry bulk:
[0088] ① Weigh 3 grams of air-dried pulp sheet, tear it into small pulp sheets of about 3 cm × 3 cm manually, and use a universal crusher to raise it into single fibers.
[0089] ② Manually spread all the raised bamboo pulp fibers evenly on a former with holes at the bottom. The bottom diameter of the former is 50 mm and the diameter of the hole is 1.5 mm.
[0090] ③ Then gently place a 500-gram weight on the upper part of the former to press down the bamboo pulp fibers. After 30 seconds, record the sample height as the fluffy height h. The dry fluffy degree is 0.655h.
[0091] Determination of water absorption and water absorption time:
[0092] After the dry bulk measurement is completed, place the former with weights and bamboo pulp fibers in a pre-filled container with an appropriate amount of 28
[0093] ℃ distilled water beaker (a stainless steel ring is placed in the beaker for easy placement of the former). Start timing when the water begins to soak the bottom of the bamboo pulp fiber layer, and stop timing after the sample is soaked. Record the water absorption time s, and take two significant figures.
[0094] After the sample has absorbed water for 30 seconds, take out the former and allow it to drip water naturally for 30 seconds. Then remove the weight on the former and weigh the net weight of the wet bamboo pulp fiber, which is the water absorption weight G. The water absorption amount is (G-3) / 3.
[0095] Determination of complete napping decomposition time:
[0096] The prepared 3g bamboo pulp board is placed in a universal high-speed pulverizer and broken into single fibers by the built-in blade rotor at a speed of 28000r / min. The rotor blade is pure angle and will not cut the fiber. Start the equipment to start timing, stop after a certain period of time, and then break the fiber.
[0097] Turn on the equipment and visually check whether the fibers are completely broken up into single fibers. If they are completely broken up into single fibers, the raising time is t1. If there are pulp lumps, continue to start the equipment to loosen them for t2 time until they are completely broken up. At this time, the raising time is t1+t2.
[0098] From the above test results, the bamboo fluff pulp boards of Examples 1, 2, and 3 have absorption properties comparable to those of existing coniferous wood fluff pulp, and their compactness, bursting resistance, dry bulkiness and other indicators are also close to those of coniferous wood fluff pulp, and are better than the bamboo fluff pulp obtained by conventional grading treatment (Comparative Examples 1-4). At the same time, the complete napping time of Examples 1-3 is comparable to that of coniferous wood fluff pulp, and is far better than the bamboo fluff pulp obtained by conventional grading treatment (Comparative Examples 1-4). All indicators are far better than those of Comparative Example 5. At the same time, compared with Comparative Example 6 that has undergone special treatment, all performance indicators are close, but the fiber utilization rate will be much greater than that of Comparative Example 6, that is, Comparative Example 6 can only utilize bamboo fibers with a fiber length of 1.65-1.9 mm, and the remaining fibers cannot be directly utilized, while in the present invention, only bamboo fibers below 0.4 mm cannot be directly utilized. In addition, by treating in this manner, different types of bamboo can obtain basically identical bamboo fluff pulp, and different types of bamboo materials can be comprehensively utilized in a complementary manner.
[0099] The above description is only an embodiment of the present application and does not limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A bamboo fluff pulp board, the complete fluffing time is less than 40s, and the density is 0.5-0.6g / cm 3 , dry bulk greater than 24cm 3 / g, the water absorption is greater than 9g / g, and the bamboo fluff pulp board comprises bamboo fibers, It is characterized in that The bamboo fibers have the following distribution according to length: Bamboo fibers smaller than 0.4 mm account for less than 1%; 0.4-0.85mm bamboo fiber 4-6.5%; Bamboo fiber ≥1.7mm accounts for 60% or more; Moreover, the proportion of kinked fibers is 57-66%.
2. The bamboo fluff pulp board according to claim 1, It is characterized in that The average length of the bamboo fibers is greater than or equal to 1.6 mm, and the proportion of broken fibers is less than or equal to 12%.
3. The bamboo fluff pulp board according to claim 2, It is characterized in that The fibers in the bamboo fluff pulp board are all bamboo fibers.
4. The bamboo fluff pulp board according to claim 2, It is characterized in that 0.4-0.85mm bamboo fiber accounts for 5.8-6.5%, and the complete fluffing time is less than 35s.
5. A method for preparing the bamboo fluff pulp board according to claim 1, It is characterized in that The steps include: S1: providing initial bamboo pulp; S2: adjusting the fiber distribution of the initial bamboo pulp to obtain the bamboo pulp to be used, wherein the bamboo fibers of less than 0.4 mm account for less than 1%; the bamboo fibers of 0.4-0.85 mm account for 4-6.5%; and the bamboo fibers of ≥1.7 mm account for greater than or equal to 60%; S3: The bamboo pulp to be used is papermade to obtain a bamboo fluff pulp board.
6. The preparation method according to claim 5, It is characterized in that Step S2 is formed in the following manner: S21: performing a first screening process on the initial bamboo pulp to obtain a first bamboo pulp having a fiber length greater than 0.85 mm and a second bamboo pulp having a fiber length less than 0.85 mm; S22: performing a second screening process on the first bamboo pulp to obtain a third bamboo pulp having a fiber length of greater than or equal to 1.7 mm and a fourth bamboo pulp having a fiber length of 0.85-1.7 mm, and performing a third screening process on the second bamboo pulp to obtain a fifth bamboo pulp having a fiber length of 0.4-0.85 mm; S23: adding the third bamboo pulp and the fifth bamboo pulp to the fourth bamboo pulp to form standby bamboo pulp, wherein the proportion of bamboo fibers with a diameter of 0.4-0.85 mm in the standby bamboo pulp is 4-6.5%, and the proportion of bamboo fibers with a diameter of 1.7 mm or larger is greater than or equal to 60%.
7. The preparation method according to claim 5, It is characterized in that After the second and third screening processes, the third bamboo pulp and the fifth bamboo pulp are transported to corresponding storage tanks, and then the third bamboo pulp and the fifth bamboo pulp in the corresponding storage tanks are transported to the pulp mixing system, and the pulp mixing system mixes the fourth bamboo pulp, the third bamboo pulp and the fifth bamboo pulp to form stand-by bamboo pulp.
8. The preparation method according to claim 6, It is characterized in that In step S23, the bamboo fibers with a diameter of 0.4-0.85 mm account for 5.8-6.5% of the bamboo pulp to be used.