A high-performance carbon-based composite thermal interface film and its preparation method
The carbon-based composite thermal interface film prepared by combining graphene and PVDF solves the problem of insufficient thermal conductivity of existing materials, and achieves efficient heat dissipation and electromagnetic shielding performance, making it suitable for high power density electronic devices.
Patent Information
- Application Number
- CN202311248408.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-25
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-09-25
AI Technical Summary
Existing thermal interface materials have limited thermal conductivity, which cannot meet the heat dissipation requirements of high power density electronic devices.
High-performance carbon-based composite thermal interface films were prepared using graphene and polyvinylidene fluoride (PVDF) as raw materials through coating and magnetron sputtering. A highly efficient thermally conductive network was constructed by combining two-dimensional graphene, one-dimensional copper nanowires and zero-dimensional boron nitride nanowires. The coating thickness was 50-300 μm. The films were then pressed into thermal interface substrates and copper films were deposited on the surface.
The prepared thermal interface film has a thermal conductivity of over 350 W/mK, possesses excellent electromagnetic shielding and mechanical properties, and is suitable for heat dissipation in high-power-density electronic devices.
Smart Images

Figure CN117402385B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the fields of thermal conductive film materials and surface science and technology, specifically a high-performance carbon-based composite thermal interface film and its preparation method. Background Technology
[0002] Heat dissipation has always been a key research area in the electronics industry. The actual operating temperature of electronic components is one of the critical factors affecting their reliability and lifespan. Studies have shown that for every 10°C increase in temperature, the failure rate of Si or GaAs semiconductors due to shortened lifespan is three times higher. This is because in microelectronic integrated circuits or high-power rectifier devices, the heat dissipation difference between materials leads to thermal fatigue and thermal stress caused by the mismatch of thermal expansion coefficients.
[0003] As electronic devices evolve towards miniaturization, high integration, and high power density, their power consumption density is gradually increasing, and the heat generated by these devices is also increasing exponentially. This places higher demands on the heat dissipation performance of the system, leading to the development of thermal interface materials. Thermal interface materials, also known as thermal interface materials or interfacial thermal conductive materials, are widely used in IC packaging and electronic heat dissipation. They are primarily used to fill micro-gaps and uneven surface pores generated when electronic devices are connected or in contact with heat sinks, reducing thermal resistance and improving the heat dissipation performance of the device.
[0004] There are many types of thermal interface materials, commonly including thermal paste, thermal gel, thermal phase change materials, thermal grease, and liquid metal. However, the thermal conductivity of these materials is very limited: the thermal conductivity of thermal paste is typically between 2-6 W / m·K; the thermal conductivity of thermal gel is about 1-3 W / m·K; the thermal conductivity of thermal phase change materials is generally between 1-3 W / m·K; the highest thermal conductivity of thermal grease is about 11 W / m·K; and the thermal conductivity of liquid metal thermal agents is several times that of traditional thermal grease, but it can only reach 73 W / m·K. Therefore, it is necessary to develop thermal interface materials with high thermal conductivity. Summary of the Invention
[0005] In view of this, the present invention provides a high-performance carbon-based composite thermal interface film and its preparation method to solve the problems mentioned in the background art. The high-performance carbon-based composite thermal interface film is prepared using graphene and polyvinylidene fluoride (PVDF) as raw materials and a coating technology that is cost-effective and easy to scale up.
[0006] To achieve the above objectives, the present invention provides the following technical solution:
[0007] This invention discloses a method for preparing a high-performance carbon-based composite thermal interface film, comprising the following steps:
[0008] (1) Dissolve polyvinylidene fluoride in an appropriate amount of N-methylpyrrolidone and stir magnetically to form a solvent;
[0009] (2) Add graphene and boron nitride to the solvent, pre-disperse, then add copper nanowires, and disperse by magnetic stirring and ultrasonication to obtain a mixed slurry; in the mixed slurry, the mass ratio of polyvinylidene fluoride, graphene, boron nitride and copper nanowires is 2:(2-12):(1-6):(1-6);
[0010] (3) The mixed slurry is coated onto the surface of the substrate layer with a coating thickness of 50-300μm, and then dried under low temperature vacuum to obtain a thermal interface substrate.
[0011] (4) The thermal interface substrate is subjected to isostatic pressing under a pressure of not less than 10 MPa to obtain a thermal interface sheet.
[0012] (5) The thermal interface sheet is subjected to high-temperature vacuum drying treatment to obtain a thermal interface film substrate; the thermal interface film substrate includes a substrate layer and a thermally conductive film attached to the surface of the substrate layer.
[0013] (6) Separate the thermal conductive film from the substrate layer and deposit a copper film with a thickness of 2-10 μm on the surface of the thermal conductive film using magnetron sputtering to obtain a carbon-based composite thermal interface film.
[0014] As a further aspect of the present invention: in step (1), the mass ratio of polyvinylidene fluoride to N-methylpyrrolidone is 3%-15%.
[0015] As a further aspect of the present invention: in step (3), the substrate layer is one of stainless steel foil, copper foil, glass, and polyimide board.
[0016] As a further aspect of the present invention: in step (4), the specific parameters of the rolling process are: pressure 10-60MPa, rolling times 3-5 times.
[0017] As a further aspect of the present invention: in step (3), the vacuum degree of the low-temperature vacuum drying is 10-50 Pa, the drying temperature is 60-90℃, and the drying time is 1-3 hours.
[0018] As a further aspect of the present invention: in step (5), the vacuum degree of the high-temperature vacuum drying is 0.1-10 Pa, the drying temperature is 100-120℃, and the drying time is 3-8 hours.
[0019] As a further aspect of the present invention, the graphene layer is no more than 5 layers.
[0020] As a further aspect of the present invention, the thickness of the thermally conductive film is 38-60 μm.
[0021] Another aspect of the present invention discloses a high-performance carbon-based composite thermal interface film, which is prepared by the preparation method described in any of the above claims.
[0022] Compared with the prior art, the beneficial effects of the present invention are:
[0023] The thermal interface film material proposed in this invention is prepared using a blade coating method, which is simple and easy to mass-produce. The resulting thermal interface film material has good flexibility, is lightweight, has low density, can be bent and folded, and can be reused in practical use. By depositing a conductive and thermally conductive copper coating on the surface of the thermally conductive film using magnetron sputtering, the "blackening" phenomenon on the surface of the carbon material thermally conductive film can be effectively prevented, while significantly improving the electromagnetic shielding performance of the thermally conductive film. The thermally conductive film uses two-dimensional sheet graphene, one-dimensional copper nanowires, and zero-dimensional boron nitride nanoparticles as high thermal conductivity fillers to construct an efficient thermally conductive network structure, increasing the entanglement between the fillers and effectively improving the thermal conductivity of the thermally conductive film.
[0024] During stirring, PVDF, with its certain viscosity, can adhere to fillers such as graphene, resulting in a more uniform dispersion of the thermally conductive fillers. PVDF acts as a binder for various thermally conductive fillers in the film, and the film's flexibility and tensile strength primarily derive from the role of PVDF within the film. Copper nanowires and nano-boron nitride have significant positive effects on the material's electronic shielding properties and thermal conductivity.
[0025] This carbon-based composite thermal interface film material has a thermal conductivity of over 350 W / mK, excellent electromagnetic shielding performance, and an EMI SE of 30-100 dB; it also has good mechanical properties, with a tensile strength of 15-50 MPa. Attached Figure Description
[0026] Figure 1 The cross-sectional morphology of the thermal interface film obtained in Example 1 as captured by scanning electron microscopy;
[0027] Figure 2 The image shows a high-performance carbon-based cross-sectional membrane photographed by a digital camera, representing the thermal interface film obtained in Example 3.
[0028] Figure 3 This is a graph showing the trend of thermal conductivity as a function of the ratio of PVDF to graphene.
[0029] Figure 4 The graph shows the trend of tensile strength as a function of the ratio of PVDF to graphene.
[0030] Figure 5 The graph shows the trend of electromagnetic shielding performance as a function of the ratio of PVDF and graphene. Detailed Implementation
[0031] To facilitate understanding of the present invention, a more comprehensive description will be given below with reference to specific embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and complete understanding of the disclosure of the present invention.
[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.
[0033] The specific information of the raw materials used in the following examples and comparative examples is as follows:
[0034] The manufacturer of polyvinylidene fluoride (PVDF) is Shanghai Aladdin Biochemical Technology Co., Ltd., and the grade is HSV900.
[0035] The graphene is manufactured by Hebei Luohong Technology Co., Ltd., with sheet diameters of 5-50μm and 2-5 layers.
[0036] The manufacturer of N-methylpyrrolidone (NMP) is Shanghai Aladdin Biochemical Technology Co., Ltd., with the brand name AR. The manufacturer of 99.0% pure nano boron nitride is Shanghai Aladdin Biochemical Technology Co., Ltd., with the specification <150nm.
[0037] The copper nanowire manufacturer is Jiangsu Xianfeng Nanomaterials Technology Co., Ltd., with a diameter of 50-200nm and a length of 1-10 micrometers.
[0038] The copper sputtering target is manufactured by Zhongnuo New Materials (Beijing) Technology Co., Ltd., and the specifications are φ25.4mm and 5mm.
[0039] All materials are commercially available, commonly used products.
[0040] The roller press used for the roller pressing process is model YEJ112M-6 (200*300mm).
[0041] The thermal conductivity in the examples and comparative examples was determined according to the following formula:
[0042] K is thermal conductivity; Cp is specific heat capacity; λ is thermal diffusivity; ρ is thermally conductive film density.
[0043] The test standard for the thermal diffusivity λ is GB / T 22588-2008, using the laser flare method, and the equipment is a NETZSCHLFA 467 laser flare meter (Germany);
[0044] Cp was determined using differential scanning calorimetry (DSC) on a DSC240 Netzsch Selb, Germany. Density was calculated using the formula ρ = m / V (mass m was measured using an analytical balance, and V was calculated by multiplying the area and thickness of the thermally conductive film).
[0045] The test temperature was room temperature (25℃). The thermally conductive film was peeled off from the substrate before the test was conducted.
[0046] It is understood that the above-mentioned raw materials and reagents are merely examples of some specific embodiments of the present invention, making the technical solution of the present invention clearer, and do not mean that the present invention can only use the above-mentioned reagents. The specific scope shall be determined by the claims. In addition, unless otherwise specified, "parts" in the examples and comparative examples refer to parts by weight.
[0047] Any range described in this invention includes the endpoint, any value between the endpoints, and any subrange consisting of the endpoint or any value between the endpoints.
[0048] Example 1
[0049] 1) Dissolve 3 parts of PVDF in 97 parts of NMP and stir magnetically to form a solvent;
[0050] 2) Graphene is added to the above solvent for pre-dispersion, and then copper nanowires and boron nitride are added to it. The mixture is then dispersed by magnetic stirring combined with ultrasound to obtain a uniform and stable slurry. The mass ratio of PVDF, graphene, copper nanowires and boron nitride in the slurry is 2:6:1:1.
[0051] 3) A coating with a thickness of 100 μm was prepared on a copper foil substrate by coating method, and then placed in a vacuum oven for pretreatment at a vacuum degree of 20 Pa, a temperature of 70 °C, and a time of 2 hours to obtain a thermal interface substrate.
[0052] 4) The above-mentioned thermal interface substrate is subjected to cold isostatic pressing under a pressure of 30 MPa to obtain a thermal interface sheet.
[0053] 5) The thermal interface sheet is dried in a vacuum oven at a vacuum degree of 0.1 Pa, a temperature of 100 °C, and a time of 3 hours to obtain a thermal interface film substrate; the thermal interface electrode sheet includes a copper foil substrate and a thermally conductive film attached to the copper foil substrate.
[0054] 6) Peel the thermally conductive film off the copper foil substrate and deposit a copper film on the surface of the thermally conductive film using magnetron sputtering. The thickness of the copper coating is 2μm, thus obtaining the carbon-based composite thermal interface film.
[0055] The carbon-based composite thermal interface film was tested and found to have a thickness of 38 μm, a thermal conductivity of 351 W / mK, an EMI SE of 46 dB, and a tensile strength of 15 MPa. EMI stands for Electromagnetic Interference, and SE stands for Shielding Efficiency.
[0056] Example 2
[0057] 1) Dissolve 5 parts of PVDF in 95 parts of NMP and stir magnetically to form a solvent;
[0058] 2) Graphene was dispersed in the above solvent for pre-dispersion, and then copper nanowires and boron nitride were added. The mixture was then dispersed using magnetic stirring combined with ultrasound to obtain a uniform and stable slurry. In this slurry, the mass ratio of PVDF, graphene, copper nanowires, and boron nitride was 1:2:1:1.
[0059] 3) A coating with a thickness of 150 μm was prepared on copper foil by coating method, and then placed in a vacuum oven for pretreatment at a vacuum degree of 20 Pa, a temperature of 70 °C, and a time of 2 hours to obtain a thermal interface substrate.
[0060] 4) The above-mentioned thermal interface substrate is subjected to cold isostatic pressing under a pressure of 20 MPa to obtain a thermal interface sheet.
[0061] 5) The obtained thermal interface sheet is dried in a vacuum oven at a vacuum degree of 0.1 Pa, a temperature of 100 °C, and a time of 3 hours to obtain a thermal interface film substrate; the thermal interface electrode sheet includes a copper foil substrate and a thermally conductive film attached to the copper foil substrate.
[0062] 6) Peel the thermally conductive film off the copper foil substrate and deposit a copper film on the surface of the thermally conductive film using magnetron sputtering. The thickness of the copper coating is 5μm, thus obtaining the carbon-based composite thermal interface film.
[0063] Tests showed that the carbon-based composite thermal interface film has a thickness of 45 μm, a thermal conductivity of 319 W / mK, an EMI SE of 43 dB, and a tensile strength of 25 MPa.
[0064] Example 3
[0065] 1) Dissolve 8 parts of PVDF in 92 parts of NMP and stir magnetically to form a solvent;
[0066] 2) Graphene is dispersed in the above solvent for pre-dispersion, and then copper nanowires and boron nitride are added to it. The dispersion is carried out by magnetic stirring combined with ultrasound to obtain a uniform and stable mixed slurry. In the mixed slurry, the mass ratio of PVDF, graphene and copper nanowires is 2:8:1:1.
[0067] 3) A coating with a thickness of 200 μm was prepared on copper foil using a coating method, and then pretreated in a vacuum oven at a vacuum degree of 20 Pa, a temperature of 70 °C, and a time of 2 hours to obtain a thermal interface substrate;
[0068] 4) Under a pressure of 30 MPa, the above-mentioned thermal interface substrate is subjected to cold isostatic pressing to obtain a thermal interface sheet.
[0069] 5) The coating is dried in a vacuum oven at a vacuum degree of 0.1 Pa, a temperature of 100 °C, and a time of 3 hours to obtain a thermal interface film substrate; the thermal interface electrode includes a copper foil substrate and a thermally conductive film attached to the copper foil substrate.
[0070] 6) Peel the thermally conductive film off the copper foil substrate and deposit a copper film on the surface of the thermally conductive film using magnetron sputtering. The thickness of the copper coating is 10 μm, thus obtaining the carbon-based composite thermal interface film.
[0071] Tests showed that the carbon-based composite thermal interface film has a thickness of 47 μm, a thermal conductivity of 410 W / mK, an EMI SE of 100 dB, and a tensile strength of 22 MPa.
[0072] Comparative Example 1
[0073] The difference between Comparative Example 1 and Example 4 is that the mass ratio of PVDF, graphene, copper nanowires and boron nitride in the solvent of Comparative Example 1 is 2:1:1:1.
[0074] Tests showed that the carbon-based composite thermal interface film has a thickness of 58 μm, a thermal conductivity of 87 W / mK, an EMI SE of 19 dB, and a tensile strength of 29 MPa.
[0075] Comparative Example 2
[0076] The difference between Comparative Example 2 and Example 4 is that the mass ratio of PVDF, graphene, copper nanowires and boron nitride in the solvent of Comparative Example 2 is 1:8:1:1.
[0077] Tests showed that the carbon-based composite thermal interface film has a thickness of 39 μm, a thermal conductivity of 266 W / mK, an EMI SE of 78 dB, and a tensile strength of 9 MPa.
[0078] Comparative Example 3
[0079] 1) Dissolve 8 parts of PVDF in 92 parts of NMP and stir magnetically to form a solvent;
[0080] 2) Graphene is dispersed in the above solvent and dispersed by magnetic stirring combined with ultrasound to obtain a uniform and stable mixed slurry; in the mixed slurry, the mass ratio of PVDF, graphene and copper nanowires is 1:4.
[0081] 3) A coating with a thickness of 200 μm was prepared on copper foil by coating method, and then placed in a vacuum oven for pretreatment at a vacuum degree of 20 Pa, a temperature of 70 °C, and a time of 2 hours to obtain a thermal interface substrate.
[0082] 4) Under a pressure of 10 MPa, the above-mentioned thermal interface substrate is subjected to cold isostatic pressing to obtain a thermal interface sheet.
[0083] 5) The thermal interface sheet is dried in a vacuum oven at a vacuum degree of 0.1 Pa, a temperature of 100 °C, and a time of 3 hours to obtain a thermal interface film substrate; the thermal interface electrode sheet includes a copper foil substrate and a thermally conductive film attached to the copper foil substrate.
[0084] 6) Peel the thermally conductive film off the copper foil substrate and deposit a copper film on the surface of the thermally conductive film using magnetron sputtering. The thickness of the copper coating is 10 μm, thus obtaining the carbon-based composite thermal interface film.
[0085] Tests showed that the carbon-based composite thermal interface film has a thickness of 78 μm, a thermal conductivity of 301 W / mK, an EMI SE of 85 dB, and a tensile strength of 19 MPa.
[0086] Although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
[0087] Therefore, the above description is only a preferred embodiment of this application and is not intended to limit the scope of this application; that is, all equivalent modifications made in accordance with the scope of the claims of this application shall be within the protection scope of the claims of this application.
Claims
1. A method for preparing a high-performance carbon-based composite thermal interface film, characterized in that, Includes the following steps: (1) Dissolve polyvinylidene fluoride in an appropriate amount of N-methylpyrrolidone and stir magnetically to form a solvent; (2) Graphene and boron nitride are added to the solvent, pre-dispersed, and then copper nanowires are added. The mixture is then magnetically stirred and ultrasonically dispersed to obtain a mixed slurry. In the mixed slurry, the mass ratio of polyvinylidene fluoride, graphene, boron nitride, and copper nanowires is 2:(2-12):(1-6):(1-6). The number of graphene layers is 2-5. The boron nitride is nano-boron nitride with a particle size <150nm. (3) The mixed slurry is coated onto the surface of the substrate layer with a coating thickness of 50-300µm, and then dried under low temperature vacuum to obtain a thermal interface substrate. (4) Under a pressure of 20-30 MPa, the thermal interface substrate is subjected to isostatic pressing to obtain a thermal interface sheet; (5) The heat interface sheet is subjected to high-temperature vacuum drying treatment to obtain the heat interface film substrate. The thermal interface film substrate includes a substrate layer and a thermally conductive film attached to the surface of the substrate layer; (6) Separate the thermal conductive film from the substrate layer and deposit a copper film with a thickness of 2-10 μm on the surface of the thermal conductive film using magnetron sputtering to obtain a carbon-based composite thermal interface film.
2. The preparation method according to claim 1, characterized in that, In step (1), the mass ratio of polyvinylidene fluoride to N-methylpyrrolidone is 3%-15%.
3. The preparation method according to claim 1, characterized in that, In step (3), the substrate layer is one of stainless steel foil, copper foil, glass, and polyimide board.
4. The preparation method according to claim 1, characterized in that, In step (3), the vacuum degree of the low-temperature vacuum drying is 10-50 Pa, the drying temperature is 60-90℃, and the drying time is 1-3 hours.
5. The preparation method according to claim 1, characterized in that, In step (5), the vacuum degree of the high-temperature vacuum drying is 0.1-10 Pa, the drying temperature is 100-120℃, and the drying time is 3-8 hours.
6. The preparation method according to claim 1, characterized in that, The thickness of the thermally conductive film is 38-60 μm.
7. A high-performance carbon-based composite thermal interface film, which is prepared by the preparation method described in any one of claims 1-6.
Citation Information
Patent Citations
Heat-conducting and insulating boron nitride polymer composite material and preparation method thereof
CN110734644A
Sandwich-structure high-thermal-conductivity composite film thermal interface material and preparation method thereof