A functionalized carbon black support, a supported electrocatalyst, and its preparation method

By preparing functionalized carbon black supports containing atomically dispersed transition metal oxide clusters, the problems of catalytic inertness and easy migration and aggregation of noble metals in traditional carbon black materials were solved, and the high efficiency, stability and activity of supported electrocatalysts were achieved.

CN117403274BActive Publication Date: 2026-11-10ZHEJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311365728.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-20
Publication Date
2026-11-10
Estimated Expiration
2043-10-20

AI Technical Summary

Technical Problem

Traditional carbon black materials are catalytically inert and have low surface defect concentrations. Precious metal catalysts are prone to migration, aggregation, and shedding during the catalytic process, leading to performance degradation of electrocatalytic devices and hindering the development of high-performance hydrogen energy conversion devices.

Method used

A functionalized carbon black carrier containing atomically dispersed transition metal oxide clusters was prepared by dispersing the first carbon black material in a solvent, adding a transition metal precursor solution, and then drying and heat-treating it. This carrier is used to stabilize the active centers of noble metals.

Benefits of technology

It improves the dispersibility of precious metals and the stability of catalysts, enhances the catalytic effect of supported electrocatalysts, avoids the migration and aggregation of precious metals during catalysis, and enhances catalytic activity and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117403274B_ABST
    Figure CN117403274B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of electrocatalysis technology, specifically relating to a functionalized carbon black support, a supported electrocatalyst, and its preparation method. The preparation method of the functionalized carbon black support includes the following steps: dispersing a first carbon black material in a solvent, adding a transition metal precursor solution, drying, subjecting the resulting powder to a first heat treatment in an oxygen-containing atmosphere, and then subjecting it to a second heat treatment in an oxygen-free atmosphere to obtain the functionalized carbon black support. This invention prepares a carbon black support with high defect density and strong metal anchoring ability, enabling strong interaction between the supported metal and the support, further stabilizing the active centers of noble metals, and preventing migration, aggregation, and detachment of noble metals during catalysis. Simultaneously, oxyphilic elements can act as co-catalysts to promote water dissociation, further regulating the binding strength of intermediates on the metal surface, thereby improving the catalytic activity and stability of the supported electrocatalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrocatalysis technology, specifically relating to a functionalized carbon black support, a supported electrocatalyst, and a preparation method thereof. Background Technology

[0002] The information disclosed in this background section is intended only to enhance understanding of the overall background of the invention and is not necessarily to be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.

[0003] Carbon materials, due to their high specific surface area, good electrical conductivity, and low cost, have become the preferred support for supported electrocatalysts and are widely used in fields such as water electrolysis and fuel cells. Carbon supports not only disperse metal active centers to improve metal atom utilization but also help regulate the electronic structure of these centers, which is crucial for constructing highly active and durable supported electrocatalysts. Currently, most research on noble metal-based electrocatalysts uses commercially available carbon black as a support, such as acetylene black and Vulcan XC-72.

[0004] However, traditional carbon black materials are almost catalytically inert, have low surface defect concentrations, and exhibit weak interactions with noble metals, thus limiting their ability to improve the performance of noble metal catalysts. Furthermore, noble metal catalytic sites are prone to migration, aggregation, and detachment during catalysis, leading to significant performance degradation and severely hindering the development of high-performance hydrogen conversion devices. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention aims to provide a functionalized carbon black support, a supported electrocatalyst, and a preparation method thereof. This invention designs a novel functionalized carbon black support that can be used to stabilize supported metal active centers, thereby ensuring that the electrocatalyst prepared based on this functionalized carbon black support maintains good catalytic activity and stability.

[0006] To achieve the above objectives, the present invention is implemented through the following technical solution: In a first aspect, the present invention provides a method for preparing a functionalized carbon black carrier, comprising the following steps: S1. Disperse the first carbon black material in a solvent to obtain a first carbon black dispersion; S2. Add a transition metal precursor solution to the first carbon black dispersion to obtain a second carbon black dispersion; S3. Dry the second carbon black dispersion, and place the resulting powder in an oxygen-containing atmosphere for the first heat treatment to obtain the initial functionalized carbon black carrier. S4. The initial functionalized carbon black carrier is placed in an oxygen-free atmosphere for a second heat treatment to obtain the functionalized carbon black carrier.

[0007] In a second aspect, the present invention provides a functionalized carbon black carrier, obtained by the preparation method described in the first aspect, wherein the functionalized carbon black carrier comprises carbon black and atomically dispersed transition metal oxide clusters.

[0008] Thirdly, the present invention provides a supported electrocatalyst of functionalized carbon black loaded with noble metal, characterized in that it comprises the functionalized carbon black support and noble metal nanomaterials as described in the second aspect.

[0009] Fourthly, the present invention provides a method for preparing a supported electrocatalyst of noble metal supported on functionalized carbon black as described in the third aspect, characterized by comprising the following steps: The prepared noble metal dispersion is compounded with the functionalized carbon black support as described in the second aspect, washed, and dried to obtain the functionalized carbon black supported noble metal supported electrocatalyst.

[0010] Fifthly, the present invention provides the application of a supported electrocatalyst of functionalized carbon black loaded with noble metals as described in the third aspect in alkaline hydrogen evolution reaction and / or hydroxide reaction.

[0011] The beneficial effects achieved by one or more technical solutions of the present invention are as follows: According to the functionalized carbon black method provided by this invention, carbon black support materials with high defect density and strong metal anchoring ability can be prepared. By mixing a first carbon black dispersion and a transition metal precursor solution, drying, and then performing a first heat treatment in an oxygen-containing atmosphere, an initial functionalized carbon black material modified with transition metal oxides is obtained. The transition metal oxides in this initial functionalized carbon black material are sub-nanometer in size. Then, the initial functionalized carbon black material is subjected to a second heat treatment in a hydrogen or argon atmosphere, which can further reduce the valence state of the transition metal elements, obtaining a functionalized carbon black support. Thus, the functionalized carbon black support obtained by this method can further stabilize the noble metal active centers, preventing migration, aggregation, and detachment of the noble metal active centers during catalysis, maintaining good dispersion of the noble metal, and thus significantly improving the catalytic effect of the supported electrocatalyst prepared based on this functionalized carbon black support. Attached Figure Description

[0012] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.

[0013] Figure 1 The XRD patterns of NiO-CB-H2, NiO-CB-Ar, NiO-CB and CB in Example 1 are shown. Figure 2The images shown are HAADF-STEM images of NiO-CB, NiO-CB-H2, and NiO-CB-Ar from Example 1. Figure 3 The TEM image of Pt / NiO-CB-H2 in Example 1; Figure 4 XPS spectra of NiO-CB-H2, NiO-CB-Ar, and NiO-CB from Example 1; Figure 5 The hydrogen evolution LSV curves for Pt / NiO-CB-H2, Pt / NiO-CB-Ar, Pt / NiO-CB, Pt / CB, and Pt / C are shown. Figure 6 LSV curves for Pt / NiO-CB-H2, Pt / NiO-CB-Ar, Pt / NiO-CB, Pt / CB and Pt / C hydroxides; Figure 7 The hydrogen evolution LSV curves for Pt / CoO-CB-H2, Pt / CoO-CB-Ar, Pt / CoO-CB, Pt / CB, and Pt / C are shown. Figure 8 LSV curves for Pt / CoO-CB-H2, Pt / CoO-CB-Ar, Pt / CoO-CB, Pt / CB, and Pt / C hydroxides. Detailed Implementation

[0014] According to a first typical embodiment of the present invention, a method for preparing a functionalized carbon black carrier includes the following steps: S1. Disperse the first carbon black material in a solvent to obtain a first carbon black dispersion; S2. Add a transition metal precursor solution to the first carbon black dispersion to obtain a second carbon black dispersion; S3. Dry the second carbon black dispersion, and place the resulting powder in an oxygen-containing atmosphere for the first heat treatment to obtain the initial functionalized carbon black carrier. S4. The initial functionalized carbon black carrier is placed in an oxygen-free atmosphere for a second heat treatment to obtain the functionalized carbon black carrier.

[0015] The first carbon black material is obtained by pretreating commercial carbon black material with nitric acid. It has high hydrophilicity and contains abundant surface defect sites. The first carbon black material can be obtained by purchase or preparation.

[0016] The solvent for the first carbon black dispersion can be water or ethanol. For example, the first carbon black material is dispersed in 30 ml of ethanol solution and then uniformly dispersed by ultrasonic treatment to obtain the first carbon black dispersion.

[0017] The inventors discovered that the initial functionalized carbon black support obtained after the first heat treatment can further reduce the valence state of the transition metal elements by undergoing a second heat treatment in a hydrogen or argon atmosphere. This allows the functionalized carbon black support to provide more active sites, which is beneficial for adsorbing and stabilizing the loaded noble metal nanomaterials.

[0018] In one or more embodiments of this implementation, the concentration of the transition metal precursor solution is 0.01-10 mol / L, the transition metal precursor includes at least one of chromium nitrate, manganese nitrate, ferric nitrate, cobalt nitrate, nickel nitrate, copper nitrate and zinc nitrate, and the ratio of the transition metal precursor to the first carbon black material is 0.1-1 mmol:1 g.

[0019] In one or more embodiments of this implementation, the temperature of the first heat treatment is 200-400 °C, and the time is 1-2 h. After the first heat treatment, the nitrate is gradually decomposed to generate transition metal oxides, which are then atomically dispersed on the carbon black carrier.

[0020] In one or more embodiments of this implementation, the method for drying the second carbon black dispersion includes stirring and heating or cooling and drying at 40-90°C. Various methods can be used to dry the second carbon black dispersion. Specifically, freeze-drying can be used to dry the second carbon black dispersion, or the second carbon black dispersion can be placed in a water bath at 40-90°C and heated and stirred to dry it into powder. During the drying process using water bath heating, continuous stirring is necessary to ensure that the transition metal is uniformly dispersed.

[0021] In one or more embodiments of this implementation, the temperature of the second heat treatment is 200-400 °C, the time is 1-2 h, and the gas atmosphere is an argon atmosphere or a hydrogen atmosphere. For example, the initial functionalized carbon black support is placed in a tube furnace, hydrogen is introduced, and it is heated to 300 °C for 1 h. During the second heat treatment, the valence state of the transition metal in the transition metal oxide decreases, thereby controlling its coordination environment, which is beneficial to improving the catalytic activity of the electrocatalyst based on the functionalized carbon black material loaded with noble metal.

[0022] However, if the temperature of the second heat treatment is higher than 400°C, the transition metal oxides will agglomerate, which is not conducive to the preparation of carbon black carriers that can stably support noble metal active centers.

[0023] In one or more embodiments of this implementation, a method for obtaining the first carbon black material is also included: Untreated carbon black was placed in a nitric acid solution of a certain concentration and subjected to condensation and reflux heating for a certain period of time. After filtration and washing until neutral, it was vacuum dried to obtain the first pretreated carbon black material.

[0024] Further, the concentration of the nitric acid solution is 6-12 M, and the reflux heating temperature is 40-90 °C. Specifically, commercial carbon black is subjected to reflux heating at 50 °C for 1 h in a 6 mol / L nitric acid solution, then filtered and washed until neutral, and dried overnight in a vacuum oven to obtain the pretreated carbon black carrier.

[0025] By pretreating commercial carbon black, its surface hydrophilicity and the number of defect sites are increased, which facilitates subsequent functionalization of the carbon black.

[0026] The preparation method of this invention enables the pollution-free, low-cost, and large-scale preparation of functionalized carbon black carriers.

[0027] A second typical embodiment of the present invention provides a functionalized carbon black carrier, which is obtained by the preparation method described in the first typical embodiment. The functionalized carbon black carrier comprises carbon black and atomically dispersed transition metal oxide clusters.

[0028] The functionalized carbon black support obtained by the preparation method provided in the first typical embodiment has atomically dispersed transition metal oxide clusters. The carbon black surface is functionalized by using atomically dispersed transition metal oxide clusters. The oxygen species in these atomically dispersed transition metal oxide clusters have higher negative charge and proton affinity, which can promote the water dissociation step and optimize the adsorption strength of hydrogen intermediates on the surface of the supported noble metal. This is beneficial to accelerating the kinetics of hydrogen evolution and hydrogen oxidation reactions, thereby helping to achieve efficient alkaline hydrogen evolution and hydrogen oxidation reactions.

[0029] Preferably, the transition metal oxide cluster is NiO. x CoO x CrO x MnO x FeO x CuO x ZnO x At least one of them is beneficial to increase the degree of surface defects of carbon black support and avoid problems such as precious metal agglomeration during catalysis.

[0030] The third typical embodiment of the present invention is a supported electrocatalyst of functionalized carbon black loaded with noble metal, comprising the functionalized carbon black support and noble metal nanomaterials as described in the second typical embodiment.

[0031] The functionalized carbon black-supported noble metal-based supported electrocatalyst exhibits high activity and stability in alkaline hydrogen evolution and hydrogen oxidation reactions. By regulating the coordination environment of the co-catalyst, and thus achieving reverse control of the active metal center, a new approach is provided for revealing the structure-activity relationship of catalysts.

[0032] Preferably, the noble metal nanomaterial is a noble metal nanoparticle, cluster, or single atom, and the noble metal includes at least one of platinum, ruthenium, iridium, rhodium, gold, silver, palladium, etc., and the mass fraction of the noble metal nanomaterial is 0.01-60 wt%.

[0033] The fourth typical embodiment of the present invention provides a method for preparing a supported electrocatalyst of noble metal supported on functionalized carbon black as described in the third typical embodiment, comprising the following steps: The prepared noble metal dispersion is compounded with the functionalized carbon black support as described in the second typical embodiment, washed, and dried to obtain the functionalized carbon black supported noble metal supported electrocatalyst.

[0034] Preferably, the noble metal dispersion is obtained by a liquid-phase reduction method, which includes the following steps: The noble metal precursor was dispersed in an ethylene glycol solution, and then a hydrothermal reaction was carried out after the addition of sodium hydroxide.

[0035] More preferably, the concentration of the noble metal precursor dispersed in the ethylene glycol solution is 1-10 g / L, the molar ratio of the noble metal precursor to sodium hydroxide is 1:1-100, the hydrothermal reaction temperature is 120-160 °C, and the hydrothermal reaction time is 1-6 h.

[0036] The fifth typical embodiment of the present invention is the application of a supported electrocatalyst of functionalized carbon black loaded with noble metals, as described in the third typical embodiment, in the alkaline hydrogen evolution reaction and / or hydroxide reaction.

[0037] The supported electrocatalyst of the present invention exhibits high activity and high durability in alkaline hydrogen evolution reaction and / or hydrogen oxidation reaction, which helps water cracking and further enables the regulation of hydrogen intermediates, thereby accelerating the kinetics of hydrogen evolution and hydrogen oxidation reaction.

[0038] To enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below with reference to specific embodiments and comparative examples.

[0039] Example 1 A NiO x The preparation method of cluster-functionalized carbon black supported platinum noble metal catalyst is as follows: (1) Pretreatment of carbon black substrate material: 2 g of commercial carbon black was dispersed in 80 ml of concentrated nitric acid, refluxed at 80 °C for 6 h, diluted to a certain concentration, filtered, centrifuged and washed until the solution pH=7, and dried under vacuum at 60 °C to obtain the unfunctionalized carbon black carrier, CB.

[0040] (2) Transition metal oxide cluster functionalized carbon black: 100 mg of the above-mentioned CB support was dispersed in 60 ml of deionized water and sonicated to achieve uniform dispersion. Then, under magnetic stirring, 170 μl of a 0.1 M nickel nitrate precursor solution was added dropwise and mixed uniformly. The solution was then heated in a water bath until dry. The resulting homogeneous mixture was heat-treated in a muffle furnace at a heating rate of 5 °C / min to 250 °C and held for 1 h to obtain NiO. x Cluster-modified functionalized carbon black substrate material, NiO-CB; the above powder was cleaned and dried as the base substrate material, and then heat-treated at 400℃ for 1 h in H2 or Ar atmosphere to obtain different NiO. x The target substrate materials for the cluster structure are NiO-CB-H2 and NiO-CB-Ar, respectively. 。

[0041] (3) Preparation method of functionalized carbon black supported platinum electrocatalyst: 10 mg of NiO-CB, NiO-CB-H2, and NiO-CB-Ar obtained in step (2) were uniformly dispersed in 20 ml of deionized water, and 1.16 ml of a 1 g / L platinum cluster dispersion was added simultaneously. The mixture was stirred overnight, and after reaction, it was washed three times by centrifugation with deionized water and ethanol. Finally, the samples were dried overnight in a vacuum oven at 60 °C. The resulting products were functionalized carbon black supported platinum electrocatalysts, namely Pt / NiO-CB, Pt / NiO-CB-H2, and Pt / NiO-CB-Ar.

[0042] Comparative Example 1 The carbon black-supported platinum catalyst (Pt / CB) obtained without the addition of transition metal precursor solution was used as a control catalyst, and the rest was the same as in Example 1.

[0043] like Figure 1 As shown, no species-related diffraction peaks appeared in the XRD patterns of NiO-CB-H2, NiO-CB-Ar, and NiO-CB, indicating that the transition metal oxides in each substrate material exist in an amorphous form.

[0044] like Figure 2 As shown in the HAADF-STEM images of NiO-CB, NiO-CB-H2, and NiO-CB-Ar, NiO clusters can be observed, all of which are sub-nanometer in size and uniformly dispersed on the carbon black support.

[0045] like Figure 3As shown in the TEM image of Pt / NiO-CB-H2, no aggregation of noble metal particles was observed at low magnification, and the average diameter of platinum particles in the functionalized carbon black supported platinum electrocatalyst was around 1.37 nm.

[0046] like Figure 4 As shown, the XPS results for NiO-CB, NiO-CB-H2, and NiO-CB-Ar show that the valence state of Ni in NiO-CB-H2 and NiO-CB-Ar is lower than that in NiO-CB, indicating that hydrogen and argon treatment conditions can further reduce the valence state of transition metals.

[0047] Using Pt / NiO-CB-H2, Pt / NiO-CB-Ar, Pt / NiO-CB prepared in Example 1, Pt / CB prepared in Control Example 1, and commercial Pt / C as electrocatalysts, alkaline hydrogen evolution reaction tests were conducted. Before the electrochemical tests, the glassy carbon electrode was continuously polished with aluminum oxide powder of different particle sizes (from largest to smallest) in a figure-eight shape, and then cleaned with ethanol and water to obtain a clean electrode surface.

[0048] Take 2 mg of the electrocatalyst as described above, 0.49 mL of ethanol, and 10 μL of Nafion (5 wt%) solution, and sonicate for 2 h to form a homogeneous slurry. Take 10 μL of the slurry and add it dropwise to a depth of 0.196 cm. 2 The metal loading on the glassy carbon electrode surface is 0.2 mg / cm³. 2 After slow drying at room temperature, the electrode was used as the working electrode for electrochemical testing. Electrochemical tests were conducted using a Chi 760E electrochemical workstation in a five-cell electrochemical cell equipped with a three-electrode system. The carbon rod and mercury / mercury oxide electrodes were used as the counter and reference electrodes, respectively, and the electrolyte was a 1 M potassium hydroxide aqueous solution. Polarization curves were measured using linear sweep voltammetry (LSV), with the working electrode rotation speed at a scan rate of 5 mV / s. -1 Prior to this test, the working electrode was first set at 100 mV s. -1 The scan rate was cyclically scanned 6 times between 0 and -0.3 V vs. RHE. The hydrogen evolution reaction current density of the Pt / NiO-CB-H2 electrocatalyst was 10 mA cm⁻¹. -2 The corresponding overpotential is 42 mV, such as Figure 5 As shown.

[0049] Using Pt / NiO-CB-H2, Pt / NiO-CB-Ar, Pt / NiO-CB prepared in Example 1, and Pt / CB and Pt / C prepared in Control Example 1 as electrocatalysts, alkaline hydroxide reaction tests were conducted. The difference from the above-mentioned hydroxide polarization curve tests was that the electrolyte was a 0.1 M potassium hydroxide solution, and hydrogen gas was continuously purged for 30 minutes until the solution was saturated before the test, while gas was continuously introduced during the test. In addition, the measured potential range was -0.1 to 0.35 V (V vs. RHE). The limiting current density of the hydroxide reaction of the Pt / NiO-CB-H2 electrocatalyst reached 2.97 mA cm⁻¹. -2 ,like Figure 6 As shown.

[0050] like Figure 5 As shown, the hydrogen evolution reaction current of the Pt / CB electrocatalyst at an overpotential of 50 mV is 4.2 mAcm. -2 The current density is significantly lower than that of Pt / NiO-CB-H2, Pt / NiO-CB-Ar, and Pt / NiO-CB electrocatalysts. Meanwhile, the limiting current density of the Pt / CB electrocatalyst in the hydrogenation reaction is 2.62 mA cm⁻¹. -2 Its performance is significantly lower than that of Pt / NiO-CB-H2, Pt / NiO-CB-Ar and Pt / NiO-CB electrocatalysts (such as...). Figure 6 (As shown). Moreover, as Figure 5 , 6 It can be seen that the electrochemical activities of Pt / NiO-CB-H2 and Pt / NiO-CB-Ar electrocatalysts are superior to those of Pt / NiO-CB electrocatalysts.

[0051] Example 2 A CoO x The preparation method of cluster-functionalized carbon black supported platinum noble metal catalyst is as follows: (1) Pretreatment of carbon black substrate material: 2 g of commercial carbon black was dispersed in 80 ml of concentrated nitric acid, refluxed at 80 °C for 6 h, diluted to a certain concentration, filtered, centrifuged and washed until the solution pH=7, and dried under vacuum at 60 °C to obtain the unfunctionalized carbon black carrier, CB.

[0052] (2) Transition metal oxide cluster functionalized carbon black: 100 mg of the above-mentioned carrier was dispersed in 60 ml of deionized water and sonicated to achieve uniform dispersion. Then, under magnetic stirring, 290 μl of a 0.1 M cobalt nitrate precursor solution was added dropwise and mixed uniformly. The solution was then heated to dryness in a 50 °C water bath. The resulting homogeneous mixture was then heat-treated in a muffle furnace at a heating rate of 5 °C / min to 250 °C and held for 30 min to obtain CoO. x Cluster-modified functionalized carbon black substrate material CoO-CB; the above powder was cleaned, dried and used as a base sample, and then heat-treated at 300 °C for 1 h in H2 and Ar atmosphere to obtain different CoO-CBs. x The target substrate materials for the cluster structure are CoO-CB-H2 and CoO-CB-Ar, respectively.

[0053] (3) Preparation method of functionalized carbon black supported platinum electrocatalyst: The 10 mg CoO-CB, CoO-CB-H2, and CoO-CB-Ar obtained in step (2) were uniformly dispersed in 20 ml of deionized water, and 1.16 ml of a 1 g / L platinum cluster dispersion was added simultaneously. The mixture was stirred overnight, and after the reaction, it was washed three times by centrifugation with water and ethanol. Finally, the samples were dried overnight in a vacuum oven at 60 °C. The resulting products were functionalized carbon black-supported platinum heterostructure catalysts, namely Pt / CoO-CB, Pt / CoO-CB-H2, and Pt / CoO-CB-Ar.

[0054] Compare with Example 2: The carbon black-supported platinum catalyst (Pt / CB) obtained without the addition of transition metal precursor solution was used as a control catalyst, and the rest was the same as in Example 2.

[0055] The methods for hydrogen evolution reaction test and hydroxide reaction test are the same as those described above.

[0056] like Figure 7 and Figure 8 It can be seen that the electrocatalytic activity of Pt / CB electrocatalyst is significantly lower than that of Pt / CoO-CB-H2, Pt / CoO-CB-Ar and Pt / CoO-CB electrocatalyst.

[0057] Example 3 A type of MnO x The preparation method of cluster-functionalized carbon black supported ruthenium noble metal catalyst is as follows: (1) Pretreatment of carbon black substrate material: 2 g of commercial carbon black was dispersed in 80 ml of concentrated nitric acid, refluxed at 80 °C for 6 h, diluted to a certain concentration, filtered, centrifuged and washed until the solution pH=7, and dried under vacuum at 60 °C.

[0058] (2) Transition metal oxide cluster functionalized carbon black: 100 mg of the above-mentioned carrier was dispersed in 60 ml of deionized water and sonicated to achieve uniform dispersion. Then, under magnetic stirring, 560 μl of a 0.1 M manganese nitrate precursor solution was added dropwise and mixed uniformly. The solution was then heated to dryness in a 50 °C water bath. The resulting homogeneous mixture was then heat-treated in a muffle furnace at a heating rate of 5 °C / min to 300 °C and held for 30 min to obtain MnO. x Cluster-modified functionalized carbon black substrate material MnO-CB; the above powder was cleaned, dried and used as a base sample, and then heat-treated at 300 ℃ for 1 h in H2 or Ar atmosphere to obtain different MnOs. x The target substrate materials for the cluster structure are MnO-CB-H2 and MnO-CB-Ar, respectively.

[0059] (3) Preparation method of functionalized carbon black supported ruthenium electrocatalyst: The 10 mg MnO-CB, MnO-CB-H2, and MnO-CB-Ar obtained in step (2) were uniformly dispersed in 20 ml of deionized water, and 1.16 ml of a noble metal dispersion prepared using hydrated ruthenium chloride as a precursor was added simultaneously. The mixture was stirred overnight, and after reaction, it was washed three times by centrifugation with water and ethanol. Finally, the sample was dried overnight in a vacuum oven at 60 °C. The resulting product was a functionalized carbon black supported ruthenium electrocatalyst.

[0060] Compare with Example 3 The carbon black-supported ruthenium composite catalyst obtained without the addition of transition metal precursor solution was used as a control catalyst, and the rest was the same as in Example 3.

[0061] The methods for hydrogen evolution reaction test and hydroxide reaction test are the same as those described above.

[0062] Example 4 A ZnO x The preparation method of cluster-functionalized carbon black supported iridium noble metal catalyst, the specific steps are as follows: (1) Pretreatment of carbon black substrate material: 2 g of commercial carbon black was dispersed in 80 ml of concentrated nitric acid, refluxed at 80 °C for 6 h, diluted to a certain concentration, filtered, centrifuged and washed until the solution pH=7, and dried under vacuum at 60 °C.

[0063] (2) Transition metal oxide cluster functionalized carbon black: 100 mg of the above-mentioned carrier was dispersed in 60 ml of deionized water and sonicated to achieve uniform dispersion. Then, under magnetic stirring, 280 μl of a 0.1 M zinc nitrate precursor solution was added dropwise and mixed uniformly. The solution was then heated to dryness in a 50 °C water bath. The resulting homogeneous mixture was then heat-treated in a muffle furnace to 300 °C at a heating rate of 5 °C / min and held for 30 min to obtain ZnO. x Cluster-modified functionalized carbon black substrate material ZnO-CB; the above powder was cleaned, dried and used as a base sample, and then heat-treated at 300 ℃ for 1 h in H2 or Ar atmosphere to obtain different ZnO. x The target substrate materials for the cluster structure are ZnO-CB-H2 and ZnO-CB-Ar, respectively.

[0064] (3) Preparation method of functionalized carbon black supported iridium electrocatalyst: The 10 mg ZnO-CB, ZnO-CB-H2, and ZnO-CB-Ar obtained in step (2) were uniformly dispersed in 20 ml of deionized water, and 1.16 ml of a noble metal dispersion prepared using iridium trichloride as a precursor was added simultaneously. The mixture was stirred overnight, and after reaction, it was washed three times by centrifugation with water and ethanol. Finally, the sample was dried overnight in a vacuum oven at 60 °C. The resulting product was a functionalized carbon black-supported iridium electrocatalyst.

[0065] Compare with Example 4: The carbon black-supported iridium composite catalyst obtained without the addition of transition metal precursor solution was used as a control catalyst, and the rest was the same as in Example 4.

[0066] The methods for hydrogen evolution reaction test and hydroxide reaction test are the same as those described above.

[0067] Example 5 A type of CrO x The preparation method of cluster-functionalized carbon black supported platinum noble metal catalyst is as follows: (1) Pretreatment of carbon black substrate material: 2 g of commercial carbon black was dispersed in 80 ml of concentrated nitric acid, refluxed at 80 °C for 6 h, diluted to a certain concentration, filtered, centrifuged and washed until the solution pH=7, and dried under vacuum at 60 °C.

[0068] (2) Transition metal oxide cluster functionalized carbon black: 100 mg of the above-mentioned carrier was dispersed in 60 ml of deionized water and sonicated to achieve uniform dispersion. Then, under magnetic stirring, 290 μl of a 0.1 M chromium nitrate precursor solution was added dropwise and mixed uniformly. The solution was then heated to dryness in a 50 °C water bath. The resulting homogeneous mixture was then heat-treated in a muffle furnace at a heating rate of 5 °C / min to 400 °C and held for 30 min to obtain CrO. x Cluster-modified functionalized carbon black substrate material CrO-CB; the above powder was cleaned, dried and used as a base sample, and then heat-treated at 350 ℃ for 2 h in H2 or Ar atmosphere to obtain different CrO x The target substrate materials for the cluster structure are CrO-CB-H2 and CrO-CB-Ar, respectively.

[0069] (3) Preparation method of functionalized carbon black supported platinum electrocatalyst: The 10 mg CrO-CB, CrO-CB-H2, and CrO-CB-Ar obtained in step (2) were uniformly dispersed in 20 ml of deionized water, and 1.16 ml of a 1 g / L platinum cluster dispersion was added simultaneously. The mixture was stirred overnight, and after the reaction, it was washed three times by centrifugation with water and ethanol. Finally, the sample was dried overnight in a vacuum oven at 60 °C. The resulting product was a functionalized carbon black supported platinum electrocatalyst.

[0070] Compare with Example 5: The preparation method of the carbon black supported platinum composite catalyst is the same as that of Control Example 1, and the hydrogen evolution reaction test and the hydroxide reaction test are the same as those described above.

[0071] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing a supported electrocatalyst of noble metal supported on functionalized carbon black, characterized in that, Includes the following steps: The noble metal dispersion was compounded with the functionalized carbon black support, washed, and dried to obtain the functionalized carbon black supported noble metal supported electrocatalyst. The precious metal dispersion was obtained by a liquid-phase reduction method, which includes the following steps: The noble metal precursor was dispersed in an ethylene glycol solution, and a hydrothermal reaction was carried out after the addition of sodium hydroxide. The preparation method of the functionalized carbon black carrier includes the following steps: S1, dispersing the first carbon black material in a solvent to obtain the first carbon black dispersion; S2. Add a transition metal precursor solution to the first carbon black dispersion to obtain a second carbon black dispersion; S3. Dry the second carbon black dispersion, and place the resulting powder in an oxygen-containing atmosphere for the first heat treatment to obtain the initial functionalized carbon black carrier. S4. The initial functionalized carbon black support is placed in an oxygen-free atmosphere for a second heat treatment to obtain the functionalized carbon black support. The temperature of the first heat treatment is 200-400 ℃, and the time is 1-2 h; The second heat treatment is performed at a temperature of 200-400 ℃ for 1-2 h. The functionalized carbon black carrier comprises carbon black and atomically dispersed transition metal oxide clusters.

2. The preparation method according to claim 1, characterized in that, The concentration of the transition metal precursor solution is 0.01-10 mol / L, and the transition metal precursor includes at least one of chromium nitrate, manganese nitrate, ferric nitrate, cobalt nitrate, nickel nitrate, copper nitrate, and zinc nitrate. The ratio of the transition metal precursor to the first carbon black material is 0.1-1 mmol:1 g.

3. The preparation method according to claim 1, characterized in that, Methods for drying the second carbon black dispersion include stirring and heating or cooling and drying at 40-90℃.

4. The preparation method according to claim 1, characterized in that, The gas atmosphere is either argon or hydrogen.

5. The preparation method according to claim 1, characterized in that, It also includes the method for obtaining the first carbon black material: Untreated carbon black was placed in a nitric acid solution for condensation and reflux heating treatment. After treatment, it was filtered, washed until neutral, and then vacuum dried to obtain the first carbon black material.

6. The preparation method according to claim 1, characterized in that, The concentration of the noble metal precursor dispersed in the ethylene glycol solution is 1-10 g / L, the molar ratio of the noble metal precursor to sodium hydroxide is 1:1-100, the hydrothermal reaction temperature is 120-160 ℃, and the hydrothermal reaction time is 1-6 h.

7. The preparation method according to claim 5, characterized in that, The concentration of the nitric acid solution is 6-12 M, and the condensation reflux heating temperature is 40-90 ℃.

8. A supported electrocatalyst of noble metal supported on functionalized carbon black, characterized in that, Obtained by the preparation method according to any one of claims 1-7; including carbon black and atomically dispersed transition metal oxide clusters of functionalized carbon black carrier and noble metal nanomaterials.

9. The supported electrocatalyst of functionalized carbon black supporting noble metals as described in claim 8, characterized in that, The noble metal nanomaterial is a noble metal cluster, and the noble metal includes at least one of platinum, ruthenium, iridium, rhodium, gold, silver and palladium, and the mass fraction of the noble metal nanomaterial is 0.01-60 wt%.

10. The application of the functionalized carbon black supported noble metal electrocatalyst as described in claim 8 in alkaline hydrogen evolution reaction and / or hydroxide reaction.