Method for detecting vertical state of side surface of photoresist dry film circuit

Through metallographic slicing sample preparation and film removal technology, the vertical state of the side of the photoresist dry film line is detected, which solves the problem that the cross-sectional shape of the photoresist dry film line cannot be accurately detected in the prior art, and improves the graphic copper plating The quality of the line and signal integrity improve the reliability and yield of the production process.

CN117412490BInactive Publication Date: 2024-11-01UNIV OF ELECTRONICS SCI & TECH OF CHINA +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311334906.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-16
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing technology cannot accurately detect the cross-sectional shape and photocuring degree of photoresist dry film lines, resulting in the quality and signal integrity of the graphic electroplating copper lines being affected, and the existing characterization methods cannot adjust the usage parameters in the production process in a timely manner, which reduces the Product yield and reliability.

Method used

Using metallographic slicing sample preparation and film removal technology, the vertical state of the side of the photoresist dry film line is measured by angle, combined with SEM scanning and Image J software measurement, accurately obtain the line cross-sectional shape information and photocuring degree, and adjust the exposure and development parameters. .

Benefits of technology

Accurate detection and imaging of photoresist dry film lines is achieved, the quality and signal integrity of graphic electroplating copper lines are improved, and the yield and reliability of fine line production are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117412490B_ABST
    Figure CN117412490B_ABST
Patent Text Reader

Abstract

The present invention provides a method for detecting the vertical state of the side of a photoresist dry film circuit, and belongs to the technical field of printed circuit board circuit manufacturing. The steps of the detection method include micro-etching of a copper-clad board, hot pressing of a photoresist dry film on the surface of the copper-clad board, selective exposure of the photoresist dry film, development to form a photoresist dry film circuit, metallographic sectioning and sample preparation, film removal of the photoresist dry film circuit, side vertical state photography, and angle measurement. In the process of pattern transfer in printed circuit board circuit manufacturing, the detection method of the present invention is adopted. After the photoresist dry film is hot pressed, exposed, and developed to form a pattern circuit on the printed circuit board, the cross-sectional shape information of the circuit can be accurately obtained, and its photocuring degree and analytical imaging capability can be judged, so as to provide guidance for setting appropriate exposure and development process parameters of the photoresist dry film in the pattern transfer, thereby ensuring the circuit quality and signal integrity of the pattern electroplated copper circuit, and improving the yield of fine circuit manufacturing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of printed circuit board circuit manufacturing, and in particular relates to a method for detecting the vertical state of the side surface of a photoresist dry film circuit. Background Art

[0002] Under the premise that consumer electronic products tend to be multifunctional and complex, the printed circuit board (PCB), which is the carrier supporting and connecting electronic components, is constantly moving towards high density, high integration, high frequency and high speed to adapt to the development of downstream electronic equipment industries. As one of the most forward-looking fine circuit manufacturing processes for PCB, the graphic refinement and reliability of the modified semi-additive process (mSAP) can meet the needs of high-end electronic products. At present, its manufacturing process is relatively mature and can be mass-produced. The mSAP process is suitable for making fine circuits of 10μm / 10μm to 50μm / 50μm. At the same time, graphic electroplating can easily control the copper thickness of the circuit to meet the low impedance requirements. Therefore, the mSAP process is used as the leading process to make fine circuits to achieve the thinness and miniaturization of electronic products and better transmission signal integrity.

[0003] Among them, as a key process in the production process of PCB fine circuits, pattern transfer includes micro-etching and copper reduction, hot pressing of photoresist dry film, exposure, development and other steps. The quality of the photoresist dry film circuit attached to the copper clad board after development will affect the signal integrity and impedance of the subsequent pattern electroplated copper circuit. For the photoresist dry film of the same formula system, different exposure light sources will show different circuit cross-sectional shapes. The main wavelength of the high-pressure mercury lamp is 365nm. The current domestic LDI equipment emission wavelength is a single wavelength of 405nm, and the penetration depth of 365nm to the photoresist layer is less than 405nm. Therefore, under the action of the high-pressure mercury lamp, the curing degree of the photoresist layer surface is greater than that of the bottom, while the latter is the opposite. The final result is that the cross-sectional shape of the photoresist dry film circuit obtained by the high-pressure mercury lamp is approximately an inverted trapezoid, while the LDI obtains a trapezoid. In addition, the photoinitiator used also affects the curing effect. If its own absorption spectrum matches the light source emission spectrum, the overall light curing degree is relatively complete, and then a photoresist dry film circuit with a vertical side wall structure can be obtained. In fact, most commercial photoinitiators on the market currently absorb below 365nm, which means that the photocuring effect of single-wavelength 405nm LDI is not ideal. Whether it is a trapezoidal or inverted trapezoidal cross-sectional shape, it affects the line quality and signal integrity of the subsequent graphic electroplated copper, and even causes impedance fluctuations that affect signal transmission. The previous method of directly characterizing the morphology of the photoresist dry film circuit through SEM cannot accurately scan the cross-sectional shape information of the photoresist dry film; and the 3D laser microscope cannot perform high-resolution imaging of 10-30μm photoresist dry film circuits. The above-mentioned characterization methods have shortcomings in judging the degree of photocuring of the photoresist dry film and the ability to analyze and image, and thus cannot timely adjust the use parameters related to the exposure and development process of the photoresist dry film in the production process, reducing the product yield and reliability. Summary of the invention

[0004] The purpose of the present invention is to address the problem of rapid and convenient characterization of the side wall structure of a fine photoresist dry film circuit, and to propose a method for detecting the vertical state of the side surface of a photoresist dry film circuit.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] A method for detecting the vertical state of the side surface of a photoresist dry film circuit comprises the following steps:

[0007] (1) Micro-etching of copper-clad laminate and hot pressing of photoresist dry film on its surface;

[0008] (2) Photoresist dry film exposure;

[0009] (3) developing to form a photoresist dry film circuit;

[0010] (4) Metallographic sectioning: Metallographic sectioning is used to fix the position and direction of the sample, exposing the cross section of the photoresist dry film circuit to the polished surface of the metallographic section, and the photoresist dry film circuit is perpendicular to the polished surface of the metallographic section;

[0011] (5) Stripping of photoresist dry film circuits: The stripping of photoresist dry film circuits is carried out by immersion method to remove the cross-sectional area of ​​the photoresist dry film circuits exposed on the polished surface of the metallographic section;

[0012] (6) Side vertical state shooting and angle measurement: After the photoresist dry film is stripped, a groove will be formed in the curing agent. After shooting the groove frame, the vertical state of each side of the cross-section of the photoresist dry film circuit is measured. The angle is the angle between the bottom edge of the frame and each side edge of the frame. The measured angle is used to determine the side vertical state of the photoresist dry film circuit.

[0013] As a preferred embodiment, the light source device of the exposure step (2) is selected from a high pressure mercury lamp and a laser, and the exposure energy range is 20 to 100 mJ / cm 2 .

[0014] As a preferred embodiment, the circuit formed by the photoresist dry film in step (3) consists of M groups of line arrays with equal line width and equal spacing, the width range of the line width or spacing is 10 to 100 μm, the line thickness range is 20 to 120 μm, and one group of arrays consists of a line and a spacing between two lines, and M is a positive integer greater than or equal to 2.

[0015] As a preferred embodiment, the development conditions in step (3) are as follows: Na2CO3 mass concentration 0.7-1.0%, development temperature 28-32°C, spray pressure 1.0-2.0 kg / cm 2 , development time 30~90s.

[0016] As a preferred embodiment, the specific process of metallographic sectioning and sample preparation in step (4) is as follows: first, the photoresist dry film circuit is cut on the XOY plane, and then the cut photoresist dry film circuit is placed in a mold, and then epoxy resin curing agent is poured into the mold and then ground and polished, and the ground and polished surface is the YOZ plane; X is defined as the extension direction of the length of the photoresist dry film circuit, Y is the extension direction of the width of the photoresist dry film circuit, and Z is the direction of the thickness of the photoresist dry film circuit.

[0017] As a preferred embodiment, the solution used for stripping the photoresist dry film circuit in step (5) is an alkaline aqueous solution containing sodium hydroxide or an organic amine.

[0018] As a preferred embodiment, the solution used for stripping the photoresist dry film circuit in step (5) is an alkaline aqueous solution containing X% by mass of sodium hydroxide or Y% by mass of an organic amine, the stripping time is 10 to 30 minutes, the stripping temperature is 40 to 60° C., and the stripping is carried out by immersion; wherein X is a positive integer greater than or equal to 2 and less than or equal to 5, and Y is a positive integer greater than or equal to 7 and less than or equal to 11.

[0019] As a preferred method, step (6) uses SEM to scan the epoxy resin curing agent framework.

[0020] As a preferred method, in step (6), the cross-sectional angle of the photoresist dry film circuit is measured by measuring the angle between the bottom edge of the curing agent frame and the side edge of the frame using Image J software to determine the side vertical state and cross-sectional shape of the photoresist dry film circuit.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention provides a method for detecting the vertical state of the side surface of a photoresist dry film circuit. In the process of pattern transfer in printed circuit board circuit manufacturing, the detection method of the present invention is adopted. After the photoresist dry film is subjected to heat pressing, exposure and development to form a pattern circuit on the printed circuit board, the cross-sectional shape information of the circuit can be accurately obtained, the degree of light curing and the analytical imaging capability can be judged, and a guiding direction is provided for setting appropriate exposure and development process parameters of the photoresist dry film in the pattern transfer, thereby ensuring the circuit quality and signal integrity of the pattern electroplated copper circuit and improving the yield rate of fine circuit manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic flow chart of a method for detecting the vertical state of the side surface of a photoresist dry film circuit of the present invention;

[0024] Figure 2 It is a three-dimensional direction marking diagram of the photoresist dry film circuit of the present invention; wherein, the XOY plane is a top view of the photoresist dry film circuit, and the YOZ plane is a cross-sectional view of the photoresist dry film circuit;

[0025] Figure 3 It is a microscopic physical image of a photoresist dry film pattern circuit obtained by conventional exposure and development without metallographic sectioning and film stripping; wherein 301 represents an XOY plane image of 7 mutually parallel 80μm / 80μm ​​circuits obtained after the photoresist dry film is exposed and developed by a laser direct imaging system (LDI), and 302 represents an XOY plane image of 7 mutually parallel 80μm / 80μm ​​circuits obtained after the photoresist dry film is exposed and developed by a high-pressure mercury lamp;

[0026] Figure 4These are SEM images of the photoresist dry film after metallographic sectioning and stripping of the present invention; wherein 401 represents a YOZ plane SEM image of an 80 μm circuit formed by the photoresist dry film after exposure and development by a laser direct imaging system (LDI), and 402 represents a YOZ plane SEM image of an 80 μm circuit formed by the photoresist dry film after exposure and development by a high-pressure mercury lamp. DETAILED DESCRIPTION

[0027] The technical solution of the present invention is described in detail below in conjunction with the accompanying drawings and embodiments.

[0028] Example 1

[0029] This embodiment provides a method for detecting the vertical state of the side surface of a photoresist dry film circuit, comprising the following steps:

[0030] (1) Micro-etching of copper-clad laminate and hot pressing of photoresist dry film on its surface;

[0031] (2) Photoresist dry film exposure;

[0032] (3) developing to form a photoresist dry film circuit;

[0033] (4) Metallographic sectioning: Metallographic sectioning is used to fix the position and direction of the sample, exposing the cross section of the photoresist dry film circuit to the polished surface of the metallographic section, and the photoresist dry film circuit is perpendicular to the polished surface of the metallographic section;

[0034] (5) Stripping of photoresist dry film circuits: The stripping of photoresist dry film circuits adopts the immersion method to remove the cross-sectional area of ​​the photoresist dry film circuits exposed on the polished surface of the metallographic section;

[0035] (6) Side vertical state shooting and angle measurement: After the photoresist dry film is stripped, a groove will be formed in the curing agent. After shooting the groove frame, the vertical state of each side of the cross-section of the photoresist dry film circuit is measured. The angle is the angle between the bottom edge of the frame and each side edge of the frame. The measured angle is used to determine the side vertical state of the photoresist dry film circuit.

[0036] Example 2

[0037] This embodiment provides a method for detecting the vertical state of the side surface of a photoresist dry film circuit, comprising the following steps:

[0038] (1) Micro-etching of copper-clad laminate and hot pressing of photoresist dry film on its surface;

[0039] (2) Photoresist dry film exposure; the light source equipment of the exposure step is selected from high pressure mercury lamp, laser and light emitting diode, and the exposure energy range is 20 to 100 mJ / cm 2 ;

[0040] (3) developing to form a photoresist dry film circuit; the circuit formed by the photoresist dry film in step (3) consists of M groups of line arrays with equal line width and equal spacing, the width of the line width or spacing ranges from 10 to 100 μm, the line thickness ranges from 20 to 120 μm, and one array consists of a line and a spacing between two lines, and M is a positive integer greater than or equal to 2. The development conditions of step (3) are: Na2CO3 mass concentration 0.7 to 1.0%, development temperature 28 to 32°C, spray pressure 1.0 to 2.0 kg / cm 2 , development time 30~90s.

[0041] (4) Metallographic sectioning: Metallographic sectioning is used to fix the position and direction of the sample, and expose the cross section of the photoresist dry film circuit on the grinding and polishing surface of the metallographic section, and the photoresist dry film circuit is perpendicular to the grinding and polishing surface of the metallographic section. The specific process of step (4) metallographic sectioning is as follows: first, the photoresist dry film circuit is cut on the XOY plane, and then the cut photoresist dry film circuit is placed in a mold, and then epoxy resin curing agent is poured into the mold and then ground and polished, and the ground and polished surface is the YOZ plane; X is defined as the extension direction of the length of the photoresist dry film circuit, Y is the extension direction of the width of the photoresist dry film circuit, and Z is the direction of the thickness of the photoresist dry film circuit.

[0042] (5) Stripping of the photoresist dry film circuit: The stripping of the photoresist dry film circuit adopts an immersion method to remove the cross-sectional area of ​​the photoresist dry film circuit exposed on the polished surface of the metallographic section; the solution used for stripping the photoresist dry film circuit in step (5) is an alkaline aqueous solution containing sodium hydroxide or an organic amine. Specifically, the solution used for stripping the photoresist dry film circuit is an alkaline aqueous solution containing a mass fraction of X% sodium hydroxide or Y% organic amine, the stripping time is 10 to 30 minutes, the stripping temperature is 40 to 60°C, and the stripping is carried out by immersion; wherein X is a positive integer greater than or equal to 2 and less than or equal to 5, and Y is a positive integer greater than or equal to 7 and less than or equal to 11.

[0043] (6) Side vertical state shooting and angle measurement: After the photoresist dry film is stripped, a groove will be formed in the curing agent. The epoxy resin curing agent frame is scanned by SEM. After shooting the groove frame, the vertical state of each side of the cross section of the photoresist dry film circuit is measured. The angle is the angle between the bottom edge of the frame and each side edge of the frame. The measured angle is used to determine the side vertical state of the photoresist dry film circuit.

[0044] Specifically, the angle between the bottom edge of the curing agent frame and the side edge of the frame is measured by Image J software to determine the vertical state and cross-sectional shape of the photoresist dry film circuit.

[0045] Example 3

[0046] This embodiment provides a method for detecting the vertical state of the side surface of a photoresist dry film circuit, the detection method comprising the following steps:

[0047] (1) Micro-etching of copper clad laminate, hot pressing of photoresist dry film on copper clad laminate; hot pressing temperature 110°C, hot pressing pressure 4.0kg / cm 2 , hot pressing speed is 1.5m / min;

[0048] (2) Then, a laser direct imaging system (LDI) was used for exposure imaging. The pattern of the exposure data was 7 photoresist dry film lines of 80 μm / 80 μm, which were completely identical in size and parallel to each other. The thickness of the photoresist dry film line was 25 μm. The exposure energy was 45 mJ / cm 2 ;

[0049] (3) After exposure, the film was left to stand for 15 minutes before development. The concentration of the developer Na2CO3 was 0.9%, the development time was 35 seconds, and the spray pressure of the developer was 1.2 kg / cm 2 , developing temperature 30℃;

[0050] (4) After development, the copper-clad laminate containing the photoresist dry film circuit pattern is cut to produce a metallographic slice,

[0051] (5) Then the film is stripped by heating and immersion, the stripping solution is 5% sodium hydroxide, and the stripping temperature is 40°C. Then the curing agent frame is scanned by SEM;

[0052] (6) The angle between the side wall of the curing agent frame and the horizontal plane of the copper clad laminate was measured by SEM photography and Image J software. The average result was 86.35°, indicating that the cross-section of the original photoresist dry film circuit was a trapezoidal structure.

[0053] Example 4

[0054] This embodiment provides a method for detecting the vertical state of the side surface of a photoresist dry film circuit, the detection method comprising the following steps:

[0055] (1) Hot press the photoresist dry film on the copper clad laminate at a temperature of 105°C and a pressure of 5.0 kg / cm 2 , hot pressing speed is 1.8m / min;

[0056] (2) Then a high-pressure mercury lamp and film are used to expose the image, with an exposure energy of 50 mJ / cm 2 ;

[0057] (3) After exposure, the film was left to stand for 15 minutes before development. The concentration of the developer Na2CO3 was 1.0%, the development time was 30 seconds, and the spray pressure of the developer was 1.2 kg / cm 2 , the developing temperature is 30°C; the pattern on the film negative is 7 photoresist dry film circuits of 80μm / 80μm ​​in parallel with each other and of the same size, and the thickness of the photoresist dry film circuit is 25μm;

[0058] (4) After development, the copper-clad laminate containing the photoresist dry film circuit pattern is cut to produce a metallographic slice,

[0059] (5) Then the film is stripped by heating and soaking, the stripping liquid is 9% organic amine solution, and the stripping temperature is 50°C. Then the curing agent frame is scanned by SEM;

[0060] (6) The angle between the side wall of the curing agent frame and the horizontal plane of the copper clad laminate was measured by SEM photography and Image J software. The average result was 96.25°, indicating that the cross-section of the original photoresist dry film circuit was an inverted trapezoidal structure.

Claims

1. A method for detecting the vertical state of the side surface of a photoresist dry film circuit, characterized in that The steps include: (1) Micro-etching of copper-clad laminate and hot pressing of photoresist dry film on its surface; (2) Photoresist dry film exposure; (3) developing to form a photoresist dry film circuit; (4) Metallographic sectioning: Metallographic sectioning is used to fix the position and direction of the sample, exposing the cross section of the photoresist dry film circuit to the polished surface of the metallographic section, and the photoresist dry film circuit is perpendicular to the polished surface of the metallographic section; (5) Stripping of photoresist dry film circuits: The stripping of photoresist dry film circuits is carried out by immersion method to remove the cross-sectional area of ​​the photoresist dry film circuits exposed on the polished surface of the metallographic section; (6) Side vertical state shooting and angle measurement: After the photoresist dry film is stripped, a groove will be formed in the curing agent. After shooting the groove frame, the vertical state of each side of the cross-section of the photoresist dry film circuit is measured. The angle is the angle between the bottom edge of the frame and each side edge of the frame. The measured angle is used to determine the side vertical state of the photoresist dry film circuit.

2. The method for detecting the vertical state of the side surface of the photoresist dry film circuit according to claim 1, characterized in that: The light source equipment of the exposure step (2) is selected from high pressure mercury lamp and laser, and the exposure energy range is 20-100 mJ / cm 2 .

3. The method for detecting the vertical state of the side surface of the photoresist dry film circuit according to claim 1, characterized in that: The circuit formed by the photoresist dry film in step (3) consists of M groups of line arrays with equal line width and equal spacing, the width range of the line width or spacing is 10 to 100 μm, the line thickness range is 20 to 120 μm, and one group of arrays consists of a line and a spacing between two lines, and M is a positive integer greater than or equal to 2.

4. The method for detecting the vertical state of the side surface of the photoresist dry film circuit according to claim 1, characterized in that: The development conditions of step (3) are: Na2CO3 mass concentration 0.7-1.0%, development temperature 28-32°C, spray pressure 1.0-2.0 kg / cm 2 , development time 30~90s.

5. The method for detecting the vertical state of the side surface of the photoresist dry film circuit according to claim 1, characterized in that: The specific process of metallographic sectioning and sample preparation in step (4) is as follows: first, the photoresist dry film circuit is cut on the XOY plane, and then the cut photoresist dry film circuit is placed in a mold, and then epoxy resin curing agent is poured into the mold and then ground and polished, and the ground and polished surface is the YOZ plane; X is defined as the extension direction of the length of the photoresist dry film circuit, Y is the extension direction of the width of the photoresist dry film circuit, and Z is the direction of the thickness of the photoresist dry film circuit.

6. The method for detecting the vertical state of the side surface of the photoresist dry film circuit according to claim 1, characterized in that: The solution used for stripping the photoresist dry film circuit in step (5) is an alkaline aqueous solution containing sodium hydroxide or organic amine.

7. The method for detecting the vertical state of the side surface of the photoresist dry film circuit according to claim 6, characterized in that: The solution used for stripping the photoresist dry film circuit in step (5) is an alkaline aqueous solution containing X% sodium hydroxide or Y% organic amine by mass, the stripping time is 10 to 30 minutes, the stripping temperature is 40 to 60° C., and the stripping is carried out in an immersion manner; wherein X is a positive integer greater than or equal to 2 and less than or equal to 5, and Y is a positive integer greater than or equal to 7 and less than or equal to 11.

8. The method for detecting the vertical state of the side surface of the photoresist dry film circuit according to claim 1, characterized in that: Step (6) uses SEM to scan the epoxy resin curing agent frame.

9. The method for detecting the vertical state of the side surface of the photoresist dry film circuit according to claim 1, characterized in that: Measurement of the cross-sectional angle of the photoresist dry film circuit in step (6): The angle between the bottom edge of the curing agent frame and the side edge of the frame is measured using Image J software to determine the side vertical state and cross-sectional shape of the photoresist dry film circuit.