Preparation and application of a highly selective chlorine evolution anode

The method of loading BiOCl on MMO electrodes solves the problems of low anode water oxidation efficiency and high cost in ammonia nitrogen wastewater treatment, achieves efficient ammonia nitrogen removal and improved selectivity of electrochemical chlorine evolution reaction, and significantly improves the economy of ammonia nitrogen wastewater treatment. sex and efficiency.

CN117417032BActive Publication Date: 2024-10-11SOUTH CHINA UNIV OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311315897.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-11
Publication Date
2024-10-11
Estimated Expiration
2043-10-11

AI Technical Summary

Technical Problem

The existing technology has problems in ammonia nitrogen wastewater treatment, such as low anode water oxidation efficiency, high cost, and competitive reactions of oxygen evolution and chlorine evolution that affect ammonia nitrogen conversion efficiency, resulting in low economy and efficiency of ammonia nitrogen wastewater treatment.

Method used

BiOCl is loaded on commercial MMO electrodes, and BiOCl@MMO electrodes are formed through electrodeposition, self-assembly and high-temperature calcination. BiOCl's catalyst layer is used to improve the reaction selectivity of the electrode interface, suppress oxygen evolution side reactions, and enhance electron transfer efficiency.

Benefits of technology

It significantly improves the removal efficiency of ammonia nitrogen in ammonia nitrogen wastewater and the selectivity of the electrochemical chlorine evolution reaction, reduces energy consumption and costs, and achieves a highly selective and highly stable ammonia nitrogen indirect oxidation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117417032B_ABST
    Figure CN117417032B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of environmental electrochemistry and discloses the preparation and application of a highly selective chlorine anode for treating ammonia nitrogen wastewater. ‑ The adsorption and activation characteristics of BiOCl are improved by using the strategy of BiOCl loading on the surface of commercial MMO electrode, using the metal catalyst layer of MMO as the ohmic contact layer to enhance electron transfer, using BiOCl as the electrocatalytic layer to improve the reaction selectivity of the electrode interface, inhibiting the oxygen evolution side reaction in the chlorine evolution process of MMO anode, and solving the problem of poor conductivity of BiOCl semiconductor materials. The designed BiOCl@MMO anode shows good removal effect in the electrochemically mediated ammonia nitrogen oxidation process. The preparation method of the present invention is simple, short in cycle and low in cost, showing the potential for large-scale industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of environmental electrochemistry, and particularly relates to the preparation and application of a highly selective chlorine evolution anode for treating ammonia nitrogen wastewater. Background Art

[0002] Ammonia nitrogen is the most harmful form of reactive nitrogen and is also one of the signs of water pollution. Its excessive discharge will pose serious risks to ecosystems and human health (such as toxicity to aquatic organisms, eutrophication of receiving water bodies, production of foul odors, and contamination of drinking water). Electrochemical water treatment technology can completely mineralize pollutants and directly utilize the input of electricity without adding additional auxiliary chemicals, making it extremely competitive in the field of environmental remediation. As a potential application to replace current water treatment technologies, it has attracted more and more research interest.

[0003] Generally, electrocatalytic ammonia nitrogen oxidation technology can be divided into direct oxidation and indirect oxidation. However, the necessary conditions for direct oxidation must at least meet two points: (i) the pH value of the reaction environment must be adjusted to greater than NH4 + pK of the acid-base pair / NH3 a value (i.e. pH>9.25), due to NH4 + It is difficult to adsorb to the anode surface, which makes it impossible to directly oxidize at the anode; (ii) a suitable anode potential is required to selectively convert its oxidation products into nitrogen gas instead of producing over-oxidation products (such as nitrogen oxides, nitrate nitrogen and nitrite nitrogen). In addition, the efficiency of anodic water oxidation is much higher than that of ammonia oxidation, and the high cost of electrodes also restricts the practical application of this technology. In the indirect oxidation process, strong oxidants such as hydroxyl radicals (HO · ) and active chlorine. The process first generates a strong oxidant on the electrode surface through an electrochemical reaction, which then diffuses into the bulk solution through various pathways and achieves the oxidation of pollutants. Related studies have shown that HO · Indirect oxidation of NH4 + -N plays a negligible role, while active chlorine is more effective in converting ammonia nitrogen.

[0004] The key to the chlorine-mediated electrochemical indirect ammonia oxidation process is the chloride ion (Cl -) by anodic oxidation. However, traditional chlorine evolution anodes, such as mixed metal oxide electrodes (Mixed metal oxide, MMO), often show lower oxygen evolution overpotentials during chlorine evolution. And the competition between oxygen evolution and chlorine evolution is mainly due to the fact that they have similar reaction mechanisms with active sites (for example, surface coordinated active oxygen). The competitive reaction of the two not only affects the conversion efficiency of ammonia nitrogen, but also has a significant impact on the current efficiency and energy consumption of the treatment system, thereby determining the economic feasibility of this technology for ammonia nitrogen wastewater treatment. Therefore, the development of a chlorine evolution anode with high selectivity and high stability is one of the key factors in achieving efficient electrochemical degradation of ammonia nitrogen wastewater. Summary of the invention

[0005] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a method for preparing a highly selective chlorine evolution electrode for indirect oxidation of ammonia nitrogen. The present invention is based on the bismuth oxychloride (BiOCl) catalyst for the Cl - Based on the adsorption and activation characteristics of BiOCl, the strategy of loading BiOCl on the surface of commercial MMO electrode was adopted, the metal catalyst layer of MMO was used as the ohmic contact layer to enhance electron transfer, and BiOCl was used as the electrocatalytic layer to improve the reaction selectivity of the electrode interface, inhibit the oxygen evolution side reaction in the chlorine evolution process of MMO anode, and solve the problem of poor conductivity of BiOCl semiconductor materials.

[0006] Another object of the present invention is to provide a highly selective chlorine evolution electrode for indirect oxidation of ammonia nitrogen prepared by the above method. The prepared anode material not only promotes the occurrence of electrochemical chlorine evolution reaction, but also can achieve efficient removal of ammonia nitrogen in wastewater.

[0007] The object of the present invention is to provide the application of the above-mentioned highly selective chlorine evolution electrode for indirect oxidation of ammonia nitrogen in the treatment of ammonia nitrogen wastewater, especially in the treatment of chlorine-containing ammonia nitrogen wastewater.

[0008] The purpose of the present invention is achieved through the following solutions:

[0009] A method for preparing a highly selective chlorine evolution anode for indirect oxidation of ammonia nitrogen comprises the following steps:

[0010] (1) subjecting a commercial MMO electrode material to an electrodeposition treatment in a bismuth salt solution by a three-electrode system or a two-electrode system to obtain an MMO electrode with a bismuth film coated on the surface (Bi@MMO);

[0011] (2) immersing the Bi@MMO electrode in a chloride-containing solution and allowing it to stand for self-assembly to obtain a BiOCl-loaded MMO electrode;

[0012] (3) The BiOCl-loaded MMO electrode is calcined at high temperature to enhance the binding property of BiOCl and MMO electrode, and then the calcined electrode is subjected to electrolysis reaction in a chlorine-containing electrolyte to obtain a highly selective chlorine evolution anode for indirect oxidation of ammonia nitrogen.

[0013] The commercial MMO electrode material described in step (1) is preferably pre-treated by washing and drying before use to remove surface organic impurities, etc. The specific steps are as follows: soak the commercial metal mixture electrode in an organic solvent and ultrasonically treat it for 5 to 10 minutes, then rinse it with water, soak it in a dilute acid solution and ultrasonically treat it for 5 to 10 minutes, and finally rinse the electrode repeatedly with deionized water and anhydrous ethanol to make the surface clean, and dry it to obtain a pre-treated metal electrode. The organic solvent includes but is not limited to at least one of acetone and ethanol; the dilute acid includes but is not limited to at least one of a hydrochloric acid solution, a sulfuric acid solution and a nitric acid solution with a hydrogen ion concentration of 0.05-0.1 mol / L.

[0014] The commercial MMO electrode material described in step (1) includes but is not limited to one of ruthenium-iridium electrode (RuO2-IrO2 / Ti), iridium-tantalum electrode (IrO2-Ta2O5 / Ti), tin-antimony electrode (SnO2-Sb / Ti), etc.; the commercial MMO electrode material includes but is not limited to plate-shaped, mesh-shaped, etc.;

[0015] The electrodeposition liquid in the electrodeposition treatment process in step (1) is a bismuth-containing salt solution, the solvent of the bismuth-containing salt solution is a mixture of ethylene glycol and water, wherein the volume ratio of ethylene glycol to water is between 1 and 3, and the bismuth salt in the bismuth-containing salt solution is at least one of bismuth nitrate, bismuth trichloride, etc.; the concentration of the bismuth-containing salt solution is 0.05 to 0.15 mol / L.

[0016] The three-electrode system described in step (1) is a three-electrode system device controlled by an electrochemical workstation, mainly comprising a working electrode, a counter electrode and a reference electrode, wherein the MMO electrode material is used as the working electrode, the counter electrode is preferably a Pt electrode, and the reference electrode is preferably an Ag / AgCl electrode;

[0017] The two-electrode system described in step (1) refers to a two-electrode system device controlled by a DC power supply, which mainly includes a cathode and an anode, wherein the Pt electrode serves as the anode and the MMO electrode material serves as the cathode.

[0018] The current density of the electrodeposition in step (1) is controlled at 3-6 mA / cm 2 , the deposition time is 3 to 6 minutes.

[0019] After the electrodeposition treatment in step (1), the product is preferably rinsed with water and dried before performing step (2), wherein the drying is preferably carried out at 60°C.

[0020] The chlorine-containing solution used for self-assembly in step (2), Cl - The concentration is between 0.5 and 1.5 mol / L, and the pH of the chlorine-containing solution is between 1.5 and 3.0; the chlorine-containing solution used for self-assembly is preferably a NaCl solution.

[0021] The temperature of the chlorine-containing solution used in the self-assembly process in step (2) is between 20 and 40° C.; the standing time is 12-36 hours.

[0022] The high temperature calcination temperature described in step (3) is 400-600° C., the calcination time is 1-3 hours, and the heating temperature is 4-6° C. / min.

[0023] The chlorine-containing electrolyte described in step (3) refers to an aqueous solution prepared from at least one of chlorine salt agents such as NaCl and KCl, wherein the concentration of chloride ions in the chlorine-containing electrolyte is 0.01-1.00 mol / L, and the pH is 5-8;

[0024] The electrolytic reaction described in step (3) refers to an electrolytic reaction with the calcined electrode as the anode and the stainless steel electrode as the cathode, wherein the electrolysis time is 1 to 5 hours and the current density is 3 to 15 mA / cm 2 Electrolysis allows BiOCl to absorb chloride ions in the solution to repair the chlorine element lost in BiOCl due to high temperature during the calcination process, so as to maintain the integrity of the BiOCl lattice.

[0025] A highly selective chlorine evolution anode for indirect oxidation of ammonia nitrogen prepared by the above method.

[0026] The above-mentioned highly selective chlorine evolution anode for indirect oxidation of ammonia nitrogen is used to remove ammonia nitrogen and other pollutants in wastewater, especially to remove ammonia nitrogen in chlorine-containing wastewater.

[0027] The mechanism of the present invention is:

[0028] The Cl atoms in BiOCl have stronger electronegativity than O atoms. Under the stimulation of the electric field, the interlayer Cl atoms are preferentially oxidized to Cl · Then Cl2 is formed. Due to the pK sp 30.75([BiO][Cl - ]=1.8×10 -31 M 2 ), thereby promoting the Cl - Towards Cl-deficient BiOCl 1-x (OH) x The reaction generates BiOCl, which greatly increases the Cl -The adsorption and activation capacity of the MMO electrode can effectively inhibit the oxygen evolution behavior at the MMO electrode interface. While obtaining the electrochemical high-efficiency chlorine evolution Faraday efficiency, it also mediates the Cl - Generate more active chlorine, thereby achieving rapid removal of ammonia nitrogen in wastewater.

[0029] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0030] (1) In the preparation method of the present invention, the metal oxide electrodes used as the substrate are all commercial electrodes, which have been mass-produced and have a wide range of sources.

[0031] (2) In the preparation method of the present invention, BiOCl used as the electrode catalyst layer has the advantages of being non-toxic, economical and readily available, environmentally friendly, and having stable properties.

[0032] (3) The BiOCl@MMO electrode prepared by the present invention uses the catalytic layer BiOCl to - The specific adsorption capacity of BiOCl@MMO anode and the ohmic contact catalyst layer on the MMO electrode surface form a heterojunction, which not only improves the selectivity of chlorine evolution reaction at the electrode interface, but also promotes the efficiency of interfacial electron transfer. The designed BiOCl@MMO anode shows good removal effect in the electrochemically mediated ammonia nitrogen oxidation process.

[0033] (4) The preparation method of the present invention is simple, has a short cycle and low cost, and shows the potential for large-scale industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a scanning electron microscope image of a commercial metal oxide electrode (taking ruthenium-iridium electrode as an example);

[0035] Figure 2 This is a scanning electron microscope image of a commercial metal oxide electrode (taking ruthenium-iridium electrode as an example) loaded with BiOCl;

[0036] Figure 3 The XRD patterns of commercial metal oxide electrodes (taking ruthenium-iridium electrodes as an example) and BiOCl@MMO;

[0037] Figure 4 For commercial metal oxide electrodes (taking ruthenium-iridium electrodes as an example) in the presence or absence of Cl - Current density voltage (LSV) scanning curve under the following conditions;

[0038] Figure 5 The BiOCl@MMO electrode in the presence or absence of Cl - Current density voltage (LSV) scanning curve under the following conditions;

[0039] Figure 6This is a comparison chart of the chlorine evolution effects of commercial metal oxide electrodes (taking ruthenium-iridium electrodes as an example) and BiOCl@MMO;

[0040] Figure 7 This is a comparison chart of the ammonia nitrogen removal effects of commercial metal oxide electrodes (taking ruthenium-iridium electrode as an example) and BiOCl@MMO. DETAILED DESCRIPTION

[0041] The present invention will be described in further detail below in conjunction with examples and drawings, but the embodiments of the present invention are not limited thereto. If specific conditions are not specified in the examples, they are carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially. The reagents used in the examples can be purchased conventionally from the market unless otherwise specified. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the art without making creative work are within the scope of protection of the present invention.

[0042] Example 1

[0043] Preparation and characterization of BiOCl@MMO electrode (taking ruthenium-iridium electrode as an example):

[0044] First, by electrodeposition (taking a two-electrode system as an example), a commercially available metal oxide electrode was used as the cathode, and a Bi metal film was electrodeposited on its surface. The Pt sheet electrode was used as the counter electrode. Bi(NO3)3·5H2O was dissolved in a mixed solution of ethylene glycol and water (EG:H2O=2:1) ​​(the concentration of Bi(NO3)3·5H2O in the mixed solution was 0.10 mol / L), and a current of 5 mA / cm was applied. 2 Direct current was used for electrodeposition. After 5 minutes, the electrode was taken out of the solution, washed with ultrapure water, and dried at 60°C to obtain the desired Bi / MMO electrode. Then, the Bi / MMO electrode was immersed in a 1 mol / L NaCl solution with a pH of 2 and a temperature of 25°C and allowed to stand for 24 hours to generate a BiOCl film on the MMO electrode by self-assembly. Subsequently, it was repeatedly washed with distilled water and ethanol solution for a few minutes and dried at 60°C. The self-assembled electrode was then heated to 500°C in air at a heating rate of 5°C / min and calcined for 120 minutes. After calcination, the prepared electrode was used as the anode and the stainless steel electrode as the cathode, and the electrolysis reaction was carried out in a 0.05 mol / L NaCl solution. The electrolysis time was 3 hours and the current density was 10 mA / cm 2 , and then dried to obtain a highly selective chlorine evolution electrode for indirect oxidation of ammonia nitrogen, referred to as BiOCl@MMO.

[0045] The surface morphology of the chlorine evolution electrode anode prepared by the above process is compared before and after. Figure 1 and Figure 2As shown, the before and after comparison of the physical structure is as follows Figure 3 As shown in the figure, it can be seen that the surface of the MMO electrode is blocky particles, but after loading BiOCl, the electrode surface is completely covered by a dense sheet structure.

[0046] In order to compare the difference in chlorine evolution performance before and after BiOCl loading, the MMO and prepared BiOCl@MMO anodes were subjected to electrochemical LSV tests in electrolytes containing 1.0M NaCl and 1.0M NaClO4, respectively, with BiOCl@MMO or MMO electrodes as working electrodes, Pt as counter electrodes, and Ag / AgCl electrodes as reference electrodes, at a scan rate of 10mV / s. Figure 4 and Figure 5 As shown, when it reaches 10mA / cm 2 At the potential required for the current density, the potentials of MMO and BiOCl@MMO anodes in NaCl electrolyte were 1.615 and 1.638 V (vs. RHE), which were significantly higher than those in NaClO4 (without Cl). - ) were 108 and 239 mV lower than that of MMO. - The LSV shift under the above conditions is significantly larger, indicating that chlorine evolution at the BiOCl@MMO anode is more favorable than that at the MMO anode in chloride-containing electrolytes.

[0047] Application Example 1:

[0048] Preparation of BiOCl@MMO anode: Same as Example 1.

[0049] At lower Cl - The cumulative amount of free chlorine generated by MMO and BiOCl@MMO anode electrochemical reaction was compared under the condition of concentration (taking 0.05 mol / L as an example): the electrolyte was prepared with NaCl at a concentration of 50 mmol / L. The experimental device consisted of a single-chamber electrolytic cell, a DC power supply, and a pair of 3×3 cm cathodes. In this system, MMO or BiOCl@MMO electrodes were used as anodes, titanium plates were used as cathodes, the distance between anodes and cathodes was 3 cm, and the reaction volume was 50 mL. A constant temperature water bath magnetic stirrer was used to maintain the constant temperature (25°C) and uniformity of the reaction solution. In the experiment, the electrochemical reaction time was 50 min, and the sampling method was interval sampling, with sampling times of 0, 10, 20, 30, 40, and 50 min, respectively. The concentration of free chlorine generated in the reaction was detected by N,N-diethyl-p-phenylenediamine (DPD) spectrophotometry.

[0050] The cumulative amount of free chlorine electrochemically generated by MMO and BiOCl@MMO anodes, such as Figure 6As shown. The free chlorine of all electrodes basically reached the cumulative equilibrium concentration within 50 minutes. The cumulative concentrations of free chlorine after the electrochemical reaction of MMO and BiOCl@MMO electrodes were 78.1 and 404 mgCl2 / L, respectively. The free chlorine yield electrochemically generated by the BiOCl@MMO anode increased by more than 5 times compared with the MMO anode without BiOCl loading. This result shows that the chlorine evolution performance of the MMO anode loaded with BiOCl is significantly improved.

[0051] Application Example 2:

[0052] Preparation of BiOCl@MMO anode: Same as Example 1.

[0053] To compare the difference between MMO and BiOCl@MMO in the degradation of ammonia nitrogen in wastewater. Simulated wastewater was set up, that is, ammonium sulfate and sodium chloride were added to ultrapure water. The initial concentration of ammonia nitrogen in the obtained 50ml simulated wastewater was 300mg / L, and the chloride ion concentration was 50mmol / L. The pH value of the simulated wastewater was adjusted with dilute sulfuric acid and sodium hydroxide solution, and the initial pH of the solution in the reactor was controlled to be 7. A DC power supply was used for constant current output mode, and the current density was 10mA / cm 2 The distance between the cathode and anode is 3 cm, and the cathode is a titanium plate. The electrochemical oxidation time is 180 min, and the sampling method is interval sampling, and the sampling times are 0, 30, 60, 90, 120, 150, and 180 min respectively.

[0054] The removal of ammonia nitrogen from wastewater by MMO and BiOCl@MMO anode electrochemical systems, such as Figure 7 As shown. Obviously, the performance of BiOCl@MMO anode electrochemical system in ammonia nitrogen removal is much better than that of MMO electrode without BiOCl loading. When MMO is used as anode, only 31.9% of ammonia nitrogen is removed after 180 minutes. When BiOCl is loaded on the MMO electrode, the removal rate of ammonia nitrogen can reach ~100% in only 150 minutes. The above results show that the degradation rate of ammonia nitrogen by MMO anode electrochemical system can be greatly improved by BiOCl loading.

[0055] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a highly selective chlorine evolution anode for indirect oxidation of ammonia nitrogen, characterized in that The following steps are involved: (1) Electrodepositing the commercial MMO electrode material in a bismuth salt solution through a three-electrode system or a two-electrode system to obtain an MMO electrode coated with a bismuth film, referred to as Bi@MMO; (2) immersing the Bi@MMO electrode in a chloride-containing solution and allowing it to stand for self-assembly to obtain a BiOCl-loaded MMO electrode; (3) The BiOCl-loaded MMO electrode is calcined at high temperature to enhance the binding property of BiOCl and MMO electrode, and then the calcined electrode is subjected to electrolysis reaction in a chlorine-containing electrolyte to obtain a highly selective chlorine evolution anode for indirect oxidation of ammonia nitrogen; The chlorine-containing solution used for self-assembly in step (2) is NaCl; The temperature of the chlorine-containing solution used in the self-assembly process in step (2) is between 20 and 40° C.; the standing time is 12-36 hours.

2. The method for preparing a highly selective chlorine evolution anode for indirect oxidation of ammonia nitrogen according to claim 1, characterized in that: The commercial MMO electrode material described in step (1) is one of a ruthenium-iridium electrode, an iridium-tantalum electrode, and a tin-antimony electrode.

3. The method for preparing a highly selective chlorine evolution anode for indirect oxidation of ammonia nitrogen according to claim 1, characterized in that: The solvent of the bismuth salt solution in step (1) is a mixture of ethylene glycol and water, wherein the volume ratio of ethylene glycol to water is between 1 and 3, and the bismuth salt in the bismuth salt solution is at least one of bismuth nitrate and bismuth trichloride; and the concentration of the bismuth salt solution is 0.05 to 0.15 mol / L.

4. The method for preparing a highly selective chlorine evolution anode for indirect oxidation of ammonia nitrogen according to claim 1, characterized in that: The three-electrode system described in step (1) is a three-electrode system device controlled by an electrochemical workstation, mainly comprising a working electrode, a counter electrode and a reference electrode, wherein the MMO electrode material is used as the working electrode, the counter electrode is a Pt electrode, and the reference electrode is an Ag / AgCl electrode; The two-electrode system described in step (1) refers to a two-electrode system device controlled by a DC power supply, which mainly includes a cathode and an anode, wherein the Pt electrode serves as the anode and the MMO electrode material serves as the cathode.

5. The method for preparing a highly selective chlorine evolution anode for indirect oxidation of ammonia nitrogen according to claim 1, characterized in that: The current density of the electrodeposition in step (1) is controlled at 3-6 mA / cm 2 , the deposition time is 3 to 6 minutes.

6. The method for preparing a highly selective chlorine evolution anode for indirect oxidation of ammonia nitrogen according to claim 1, characterized in that: The chlorine-containing solution used for self-assembly in step (2), Cl - The concentration is between 0.5 and 1.5 mol / L, and the pH of the chlorine-containing solution is between 1.5 and 3.

0.

7. The method for preparing a highly selective chlorine evolution anode for indirect oxidation of ammonia nitrogen according to claim 1, characterized in that: The high temperature calcination temperature described in step (3) is 400-600° C., the calcination time is 1-3 hours, and the heating temperature is 4-6° C. / min.

8. The method for preparing a highly selective chlorine evolution anode for indirect oxidation of ammonia nitrogen according to claim 1, characterized in that: The chlorine-containing electrolyte described in step (3) refers to an aqueous solution prepared from at least one of NaCl and KCl, wherein the concentration of chloride ions in the chlorine-containing electrolyte is 0.01 to 1.00 mol / L, and the pH is 5 to 8; The electrolytic reaction described in step (3) refers to an electrolytic reaction with the calcined electrode as the anode and the stainless steel electrode as the cathode, wherein the electrolysis time is 1 to 5 hours and the current density is 3 to 15 mA / cm 2 .

9. A highly selective chlorine evolution anode for indirect oxidation of ammonia nitrogen prepared by the method of any one of claims 1 to 8.

10. Use of the highly selective chlorine evolution anode for indirect oxidation of ammonia nitrogen according to claim 9 in the removal of ammonia nitrogen from wastewater.

11. Use of the highly selective chlorine evolution anode for indirect oxidation of ammonia nitrogen according to claim 9 in the removal of ammonia nitrogen from chlorine-containing wastewater.

Citation Information

Patent Citations

  • Electrochemistry preparation method for flaky nanometer bismuth oxychloride film photocatalyst

    CN102744087A

  • Electrochemically modified bismuth vanadate-molybdenum sulfide-cobaltosic oxide catalytic electrode, as well as preparation method and application thereof

    CN109589993A

  • Method for strengthening chlorine evolution and efficiently mineralizing ammonia nitrogen through metal electron-deficient configuration electroanode

    CN115947422A

  • Method and device for in-situ generation of Fe (IV) and wastewater treatment

    CN116177764A

  • Bismuth-based chloride-storage electrodes

    US20180201524A1