A kind of high-efficiency polyvinyl butyral resin and preparation method thereof

By using modified polyvinyl alcohol and dipentaerythritol in the preparation of polyvinyl butyral resin, the adverse phenomena of resin during processing, complex processes and waste of water resources are solved, and efficient and environmentally friendly production processes and performance are achieved. promote.

CN117417469BActive Publication Date: 2024-11-15JIANGXI HONGFENG PLASTIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311557458.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-21
Publication Date
2024-11-15
Estimated Expiration
2043-11-21

AI Technical Summary

Technical Problem

The existing polyvinyl butyral resins are prone to yellowing and hardening during processing, and the traditional preparation methods are complex, requiring a large amount of water resources, high cost, and performance needs to be improved.

Method used

Use modified polyvinyl alcohol and dipentaerythritol as additives to prepare high-efficiency polyvinyl butyral resin through catalytic reactions to avoid adding emulsifiers, use the good emulsification and dispersion properties of modified polyvinyl alcohol, reduce the washing steps, and improve the weather resistance of the resin. sex.

Benefits of technology

It has achieved the reduction of production costs, saving water resources, improving the weather resistance and performance of resins, simplifying the process, avoiding a large amount of water washing process, and protecting the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004561581270000091
    Figure BDA0004561581270000091
  • Figure BDA0004561581270000092
    Figure BDA0004561581270000092
  • Figure BDA0004561581270000101
    Figure BDA0004561581270000101
Patent Text Reader

Abstract

The present invention relates to the field of resin technology, and in particular to a high-efficiency polyvinyl butyral resin and a preparation method thereof. The high-efficiency polyvinyl butyral resin comprises polyvinyl alcohol, n-butyraldehyde, acid, modified polyvinyl alcohol, dipentaerythritol and water. The present invention also provides a preparation method thereof. Compared with the prior art, the present invention provides a high-efficiency polyvinyl butyral resin, which does not require the addition of an emulsifier during the production process. In the present invention, polyvinyl alcohol and n-butyraldehyde are used as raw materials, and modified polyvinyl alcohol and dipentaerythritol are used as additives. The polyvinyl butyral resin is prepared by catalytic reaction, and the modified polyvinyl alcohol is used to replace the emulsifier added in the production of traditional polyvinyl butyral. The modified polyvinyl alcohol itself has good dispersing and emulsifying properties, and avoids the process of removing the emulsifier by washing with a large amount of water during the production process. The preparation method provided by the present invention saves the process of washing with a large amount of water, saves a large amount of water resources, reduces production costs, and protects the environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of resins, and in particular to a high-efficiency polyvinyl butyral resin and a preparation method thereof. Background Art

[0002] Polyvinyl butyral (PVB) resin is a white solid particle with good optical properties. It is widely used in aviation, automobile, construction, photovoltaic, coating, textile, glass interlayer and other fields.

[0003] With the rapid development of the construction, automobile, photovoltaic and other industries, the demand for high-performance and high-efficiency polyvinyl butyral resins is gradually increasing. However, PVB resins must be continuously treated at relatively high temperatures (150-200°C) during the processing of safety glass interlayers. During this process, due to aging and degradation of the PVB resin, self-polymerization and oxidation of residual butyraldehyde, yellowing and hardening may occur.

[0004] Polyvinyl butyral is produced by the polymerization of polyvinyl alcohol and butyraldehyde under acid catalysis. The degree of crosslinking is difficult to control during the polymerization process and the quality of the resin cannot be guaranteed. Currently, major domestic manufacturers control polyvinyl butyral resin by adding emulsifiers, but the emulsifier requires a large amount of water in the subsequent processing process, which is costly and complex.

[0005] CN105001357A discloses a continuous preparation method of polyvinyl butyral resin catalyzed by organic acid, which is characterized by: preparing 500 parts by mass of polyvinyl alcohol-n-butyraldehyde aqueous emulsion, and continuously putting it into a high shear mixer with 100 parts by mass of 2.5% organic acid aqueous solution at the same time, and mixing for 50 seconds. -1 -150S -1 The shear rate, shear force of 50Pa-150Pa, mixing and reacting at 30℃-40℃ for 10min-20min, are sent to an aging kettle, and then reacted at 39-41℃ for 3-4h in the first stage and 59-61℃ for 2-3h in the second stage to complete the polymerization process; the mother liquor is removed by a centrifuge, and the solid is washed with water, alkali, water and dried to obtain a powdered polyvinyl butyral resin; the present invention is continuously prepared, with high efficiency, low energy consumption and stable product quality; the prepared polyvinyl butyral resin is suitable for photovoltaic packaging materials, building safety glass, automotive safety glass and other fields. However, the process is complicated, requires a large amount of water washing, wastes a lot of water resources, and the performance needs to be further improved. Summary of the invention

[0006] To achieve the above object, the present invention provides a high-efficiency polyvinyl butyral resin, which is characterized by comprising polyvinyl alcohol, n-butyraldehyde, acid, modified polyvinyl alcohol, dipentaerythritol and water.

[0007] Further preferably, the high-efficiency polyvinyl butyral resin is composed of the following raw materials in parts by weight:

[0008] Polyvinyl alcohol 50-100 parts by weight

[0009] 10-50 parts by weight of n-butyraldehyde

[0010] Acid 5-10 parts by weight

[0011] 1-6 parts by weight of modified polyvinyl alcohol

[0012] Dipentaerythritol 5-8 parts by weight

[0013] Water 300-600 parts by weight

[0014] The acid is a mixture of one or more of hydrochloric acid, sulfuric acid, nitric acid, acetic acid, phosphoric acid, and perchloric acid;

[0015] The concentration of the acid is 10-40wt%;

[0016] The preparation method of the modified polyvinyl alcohol comprises the following steps:

[0017] Add 2-3 parts by weight of polyvinyl alcohol to 50-80 parts by weight of water and soak for 30-60 minutes, then add 1-10 parts by weight of 5-10wt% sodium hydroxide solution, heat to 60-80°C and react for 40-80 minutes, then add 1-2 parts by weight of modifier, keep 60-80°C and react for 2-3 hours. After the reaction is completed, treat with reduced pressure distillation and dry to obtain modified polyvinyl alcohol.

[0018] The preparation method of the modifier comprises the following steps:

[0019] 3-6 parts by weight of alkyl diamine are added to 80-120 parts by weight of methanol and mixed evenly to obtain an alkyl diamine solution; 25-33 parts by weight of 2,3-epoxypropyltrimethylammonium chloride are added to 40-60 parts by weight of methanol and mixed evenly to obtain a 2,3-epoxypropyltrimethylammonium chloride solution; the 2,3-epoxypropyltrimethylammonium chloride solution is added to the alkyl diamine solution, heated to 80-90°C and reacted for 4-6 hours. After the reaction is completed, methanol is distilled off under reduced pressure, crystallized, filtered and dried to obtain a modifier.

[0020] The alkyl diamine is at least one of nonane diamine and decanediamine.

[0021] The present invention is not specifically limited to polyvinyl alcohol, and the polyvinyl alcohol well known in the art includes, but is not limited to, PVA1788, PVA1799, PVA1792, PVA1048, PVA1099, PVA0580, and PVA1588.

[0022] The invention uses alkyl diamine and 2,3-epoxypropyltrimethylammonium chloride as raw materials to prepare a modifier, and uses the modifier to modify polyvinyl alcohol, which has good emulsification and dispersibility. The polyvinyl alcohol has low cost, and its water solubility is enhanced after modification, and a small amount of polyvinyl alcohol can achieve a satisfactory emulsification effect. At the same time, the modified polyvinyl alcohol is used to replace the emulsifier added in the traditional polyvinyl butyral production, and the modified polyvinyl alcohol itself has good dispersibility and emulsification performance, thereby avoiding a process of removing the emulsifier by washing with a large amount of water during the production process.

[0023] The invention provides a high-efficiency polyvinyl butyral resin, which does not need to be added with an emulsifier in the production process. In the invention, polyvinyl alcohol and n-butyraldehyde are used as raw materials, and modified polyvinyl alcohol and dipentaerythritol are used as additives. The polyvinyl butyral resin is prepared through a catalytic reaction. The modified polyvinyl alcohol is used to replace the emulsifier added in the traditional polyvinyl butyral production. The modified polyvinyl alcohol has good dispersing and emulsifying properties, and a process of removing the emulsifier by washing with a large amount of water in the production process is avoided. The introduction of dipentaerythritol greatly improves the branching degree of the polyvinyl butyral, thereby improving the weather resistance of the product.

[0024] The preparation method provided by the invention saves a large amount of water washing processes, saves a large amount of water resources, reduces production costs and protects the environment.

[0025] The application also discloses a method for preparing high-efficiency polyvinyl butyral resin.

[0026] A method for preparing a high-efficiency polyvinyl butyral resin comprises the following steps:

[0027] Step 1, adding polyvinyl alcohol to water and mixing evenly, then adding modified polyvinyl alcohol and mixing evenly to obtain a mixed solution;

[0028] Step 2, add 1 / 3-1 / 2 of the formula amount of n-butyraldehyde to the above mixed solution and mix evenly, heat to 80-90°C, add 1 / 3-1 / 2 of the formula amount of acid, keep 80-90°C to continue the reaction for 2-4h, and cool to 25-35°C;

[0029] Step 3, continue to add dipentaerythritol and the remaining n-butyraldehyde, heat to 65-80°C, add the remaining acid, continue the reaction for 1-2h, cool to room temperature after the reaction is completed, filter the precipitate, wash with water, soak it in 5-10wt% sodium hydroxide aqueous solution for 30-60min, then wash with water and dry to obtain a high-efficiency polyvinyl butyral resin.

[0030] In the present application, a stepwise condensation reaction is adopted and dipentaerythritol is added at the same time to make the polyvinyl butyral have good weather resistance.

[0031] Beneficial effects of the present invention:

[0032] The invention provides a high-efficiency polyvinyl butyral resin, which does not require the addition of an emulsifier during the production process. In the invention, polyvinyl alcohol and n-butyraldehyde are used as raw materials, and modified polyvinyl alcohol and dipentaerythritol are used as additives. The polyvinyl alcohol butyral resin is prepared by catalytic reaction. The modified polyvinyl alcohol is used to replace the emulsifier added in the traditional polyvinyl butyral production. The modified polyvinyl alcohol itself has good dispersibility and emulsification properties, and avoids the process of removing the emulsifier by washing with a large amount of water during the production process. The preparation method provided by the invention saves a large amount of water washing process, saves a large amount of water resources, reduces production costs, and protects the environment. DETAILED DESCRIPTION

[0033] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0034] Introduction of the raw materials used in the embodiments of the present invention:

[0035] The polyvinyl alcohol used in the examples is PVA1788.

[0036] The following will be combined with the specific embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Example 1

[0038] A high-efficiency polyvinyl butyral resin is composed of the following raw materials in parts by weight:

[0039] Polyvinyl alcohol 100 parts by weight

[0040] 40 parts by weight of n-butyraldehyde

[0041] 20wt% hydrochloric acid 6 parts by weight

[0042] Water 600 parts by weight

[0043] The preparation method of the high-efficiency polyvinyl butyral resin comprises the following steps:

[0044] Step 1, adding polyvinyl alcohol into water and mixing evenly to obtain a polyvinyl alcohol aqueous solution;

[0045] Step 2, add 1 / 2 n-butyraldehyde to the polyvinyl alcohol aqueous solution, heat to 85°C, add 1 / 2 hydrochloric acid, keep the temperature at 85°C and continue the reaction for 3 hours, then cool to 25°C;

[0046] Step 3, continue to add the remaining n-butyraldehyde, heat to 80°C, add the remaining hydrochloric acid, continue the reaction for 1 hour, cool to room temperature after the reaction is completed, filter the precipitate, wash with water, soak it in 5wt% sodium hydroxide aqueous solution for 60 minutes, then wash with water and dry to obtain high-efficiency polyvinyl butyral resin.

[0047] Example 2

[0048] A high-efficiency polyvinyl butyral resin is composed of the following raw materials in parts by weight:

[0049] Polyvinyl alcohol 100 parts by weight

[0050] 40 parts by weight of n-butyraldehyde

[0051] 20wt% hydrochloric acid 6 parts by weight

[0052] 5 parts by weight of modified polyvinyl alcohol

[0053] 5 parts by weight of dipentaerythritol

[0054] Water 600 parts by weight

[0055] The preparation method of the modified polyvinyl alcohol comprises the following steps:

[0056] S1. Add 5 parts by weight of decanediamine to 100 parts by weight of methanol and mix them evenly to obtain a decanediamine solution; add 32.1 parts by weight of 2,3-epoxypropyltrimethylammonium chloride to 50 parts by weight of methanol and mix them evenly to obtain a 2,3-epoxypropyltrimethylammonium chloride solution; add the 2,3-epoxypropyltrimethylammonium chloride solution to the decanediamine solution, heat to 90° C. and react for 6 hours. After the reaction is completed, remove methanol by distillation under reduced pressure, crystallize, filter, and dry to obtain a modifier;

[0057] S2, add 3.2 parts by weight of polyvinyl alcohol to 50 parts by weight of water and soak for 60 minutes, then add 8 parts by weight of 5wt% sodium hydroxide aqueous solution, heat to 80°C and react for 80 minutes, then add 1.5 parts by weight of the modifier of step S1, keep the temperature at 80°C and react for 3 hours. After the reaction is completed, distill under reduced pressure and dry to obtain modified polyvinyl alcohol.

[0058] A method for preparing a high-efficiency polyvinyl butyral resin comprises the following steps:

[0059] Step 1, adding polyvinyl alcohol to water and mixing evenly, then adding modified polyvinyl alcohol and mixing evenly to obtain a mixed solution;

[0060] Step 2, add 1 / 2 of the formula amount of n-butyraldehyde to the above mixed solution and mix evenly, heat to 85°C, add 1 / 2 of the formula amount of hydrochloric acid, maintain 85°C and continue to react for 3 hours, and cool to 25°C;

[0061] Step 3, continue to add dipentaerythritol and the remaining n-butyraldehyde, heat to 80°C, add the remaining hydrochloric acid, continue the reaction for 1 hour, cool to room temperature after the reaction is completed, filter the precipitate, wash it with water, soak it in 5wt% sodium hydroxide aqueous solution for 60 minutes, then wash it with water and dry it to obtain a high-efficiency polyvinyl butyral resin.

[0062] Example 3

[0063] A high-efficiency polyvinyl butyral resin is composed of the following raw materials in parts by weight:

[0064] Polyvinyl alcohol 100 parts by weight

[0065] 40 parts by weight of n-butyraldehyde

[0066] 20wt% hydrochloric acid 6 parts by weight

[0067] 5 parts by weight of dipentaerythritol

[0068] Water 600 parts by weight

[0069] A method for preparing a high-efficiency polyvinyl butyral resin comprises the following steps:

[0070] Step 1, adding polyvinyl alcohol into water and mixing evenly to obtain a polyvinyl alcohol aqueous solution;

[0071] Step 2, add 1 / 2 of the formula amount of n-butyraldehyde to the polyvinyl alcohol aqueous solution, heat to 85°C, add 1 / 2 of the formula amount of hydrochloric acid, maintain 85°C and continue the reaction for 3 hours, then cool to 25°C;

[0072] Step 3, continue to add dipentaerythritol and the remaining n-butyraldehyde, heat to 80°C, add the remaining hydrochloric acid, continue the reaction for 1 hour, cool to room temperature after the reaction is completed, filter the precipitate, wash it with water, soak it in 5wt% sodium hydroxide aqueous solution for 60 minutes, then wash it with water and dry it to obtain a high-efficiency polyvinyl butyral resin.

[0073] Example 4

[0074] A high-efficiency polyvinyl butyral resin is composed of the following raw materials in parts by weight:

[0075] Polyvinyl alcohol 100 parts by weight

[0076] 50 parts by weight of n-butyraldehyde

[0077] 20wt% hydrochloric acid 10 parts by weight

[0078] 6 parts by weight of modified polyvinyl alcohol

[0079] Dipentaerythritol 8 parts by weight

[0080] Water 600 parts by weight

[0081] The preparation method of the modified polyvinyl alcohol is consistent with the preparation method in Example 2.

[0082] A method for preparing a high-efficiency polyvinyl butyral resin comprises the following steps:

[0083] Step 1, adding polyvinyl alcohol to water and mixing evenly, then adding modified polyvinyl alcohol and mixing evenly to obtain a mixed solution;

[0084] Step 2, add 1 / 2 of the formula amount of n-butyraldehyde to the above mixed solution and mix evenly, heat to 85°C, add 1 / 2 of the formula amount of hydrochloric acid, maintain 85°C and continue to react for 3 hours, and cool to 25°C;

[0085] Step 3, continue to add dipentaerythritol and the remaining n-butyraldehyde, heat to 80°C, add the remaining hydrochloric acid, continue the reaction for 1 hour, cool to room temperature after the reaction is completed, filter the precipitate, wash it with water, soak it in 5wt% sodium hydroxide aqueous solution for 60 minutes, then wash it with water and dry it to obtain a high-efficiency polyvinyl butyral resin.

[0086] Example 5

[0087] A high-efficiency polyvinyl butyral resin is composed of the following raw materials in parts by weight:

[0088] Polyvinyl alcohol 100 parts by weight

[0089] 10 parts by weight of n-butyraldehyde

[0090] 20wt% hydrochloric acid 5 parts by weight

[0091] 1 part by weight of modified polyvinyl alcohol

[0092] 5 parts by weight of dipentaerythritol

[0093] Water 600 parts by weight

[0094] The preparation method of the modified polyvinyl alcohol is consistent with the preparation method in Example 2.

[0095] A method for preparing a high-efficiency polyvinyl butyral resin comprises the following steps:

[0096] Step 1, adding polyvinyl alcohol to water and mixing evenly, then adding modified polyvinyl alcohol and mixing evenly to obtain a mixed solution;

[0097] Step 2, add 1 / 2 of the formula amount of n-butyraldehyde to the above mixed solution and mix evenly, heat to 85°C, add 1 / 2 of the formula amount of hydrochloric acid, maintain 85°C and continue to react for 3 hours, and cool to 25°C;

[0098] Step 3, continue to add dipentaerythritol and the remaining n-butyraldehyde, heat to 80°C, add the remaining hydrochloric acid, continue the reaction for 1 hour, cool to room temperature after the reaction is completed, filter the precipitate, wash it with water, soak it in 5wt% sodium hydroxide aqueous solution for 60 minutes, then wash it with water and dry it to obtain a high-efficiency polyvinyl butyral resin.

[0099] Test Example 1

[0100] The acid value of the high-efficiency polyvinyl butyral resin prepared in the example was tested with reference to GB / T2895-2008 "Determination of Partial Acid Value and Total Acid Value of Plastic Polyester Resins";

[0101] The high-efficiency polyvinyl butyral resin prepared in the example was tested for butyraldehyde group with reference to GB / T12688.5-2019 "Test methods for industrial styrene - Part 5: Titration method for determination of total aldehyde content";

[0102] The viscosity of the high-efficiency polyvinyl butyral resin prepared in the example was tested with reference to GB / T1723-1993 "Determination of Coating Viscosity";

[0103] The haze test of the high-efficiency polyvinyl butyral resin prepared in the example was performed with reference to GB2410-2008 "Determination of light transmittance and haze of transparent plastics";

[0104] The melt index test of the high-efficiency polyvinyl butyral resin prepared in the example was carried out with reference to GB / T3682.1-2018 "Determination of melt mass flow rate (MFR) and melt volume flow rate (MVR) of plastic thermoplastics Part 1: Standard method";

[0105] Table 1 Test results of high-efficiency polyvinyl butyral resin performance

[0106]

[0107] As shown in Table 1, the acid value of the high-efficiency polyvinyl butyral resin prepared by the present invention is ≤0.05 mgKOH / g, the butyraldehyde content is ≤71-77%, the viscosity is 98-130S, the haze is ≤0.4, and the melt index is 0.9-1.3 g / 10min.

[0108] Test Example 2

[0109] 80 parts by weight of the high-efficiency polyvinyl butyral resin prepared in each embodiment and 0.05 parts by weight of antioxidant 1010 were added to a mixer, stirred at 1000 rpm for 20 minutes, and the material temperature was controlled at 50°C; finally, 21 parts by weight of triethylene glycol diisooctanoate were added at 20 rpm and stirred for 10 minutes. Then, the mixture was put into a twin-screw extruder, the screw temperature was set at 150°C, the mold temperature was set at 165°C, and plasticization, casting, cooling, molding and winding were performed in sequence to obtain a PVB film with uniform thickness.

[0110] Refer to GB / T32020-2015 for tensile strength and elongation at break tests;

[0111] Table 2 Test results of mechanical properties of polyvinyl butyral resin film

[0112]

[0113]

[0114] Test Example 3

[0115] The PVB film prepared in Test Example 2 was cut into 400mm×400mm, respectively clamped between two pieces of glass with clean surfaces, sealed in a silica gel bag, evacuated for 15 minutes at a vacuum degree of 2.5KPa, heated to 90°C and evacuated for 15 minutes, then placed in an autoclave and hot-pressed at a pressure of 1.3MPa and 135°C for 30 minutes, and kept warm for 2 hours to make PVB laminated glass.

[0116] Refer to GB / T2680-2021 "Determination of visible light transmittance, direct sunlight transmittance, total solar energy transmittance, ultraviolet transmittance and related window glass parameters of architectural glass" for light transmittance test;

[0117] Table 3 Transmittance test results

[0118] Light transmittance / % Example 1 76.39 Example 2 91.24 Example 3 83.67 Example 4 88.40 Example 5 86.15

[0119] It can be seen from Tables 2-3 that the PVB film and PVB laminated glass prepared with the high-efficiency polyvinyl butyral resin obtained in Example 2 have good mechanical properties and light transmittance, respectively; the present invention uses alkyl diamine and 2,3-epoxypropyltrimethylammonium chloride as raw materials to prepare the modifier, and uses the modifier to modify polyvinyl alcohol, which has good emulsification and dispersibility; wherein the polyvinyl alcohol has low cost, and its water solubility is enhanced after modification, and a small amount can also achieve a satisfactory emulsification effect, and at the same time, the modified polyvinyl alcohol is used to replace the emulsifier added in the traditional polyvinyl butyral production, which itself has good dispersibility and emulsification properties, avoiding the process of removing the emulsifier by large amounts of water washing during the production process.

[0120] The invention provides a high-efficiency polyvinyl butyral resin, which does not need to be added with an emulsifier in the production process. In the invention, polyvinyl alcohol and n-butyraldehyde are used as raw materials, and modified polyvinyl alcohol and dipentaerythritol are used as additives. The polyvinyl butyral resin is prepared through a catalytic reaction. The modified polyvinyl alcohol is used to replace the emulsifier added in the traditional polyvinyl butyral production. The modified polyvinyl alcohol has good dispersing and emulsifying properties, and a process of removing the emulsifier by washing with a large amount of water in the production process is avoided. The introduction of dipentaerythritol greatly improves the branching degree of the polyvinyl butyral, thereby improving the weather resistance of the product.

[0121] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A high-efficiency polyvinyl butyral resin, Features: Polyvinyl alcohol 50-100 parts by weight 10-50 parts by weight of n-butyraldehyde Acid 5-10 parts by weight 1-6 parts by weight of modified polyvinyl alcohol Dipentaerythritol 5-8 parts by weight 300-600 parts by weight of water; The preparation method of the modified polyvinyl alcohol comprises the following steps: Add polyvinyl alcohol into water for soaking, then add sodium hydroxide solution, heat for reaction, then add modifier, keep reacting, after the reaction is finished, perform vacuum distillation for treatment, and dry to obtain modified polyvinyl alcohol; The preparation method of the modifier comprises the following steps: Add alkyldiamine to methanol and mix evenly to obtain alkyldiamine solution; add 2,3-epoxypropyltrimethylammonium chloride to methanol and mix evenly to obtain 2,3-epoxypropyltrimethylammonium chloride solution; add 2,3-epoxypropyltrimethylammonium chloride solution to alkyldiamine solution, heat to react, after the reaction is completed, remove methanol by reduced pressure distillation, crystallize, filter and dry to obtain a modifier.

2. The high-efficiency polyvinyl butyral resin according to claim 1, Features: The acid is a mixture of one or more of hydrochloric acid, sulfuric acid, nitric acid, acetic acid, phosphoric acid and perchloric acid.

3. The high-efficiency polyvinyl butyral resin according to claim 2, Features: The concentration of the acid is 10-40 wt %.

4. A method for preparing a high-efficiency polyvinyl butyral resin as claimed in any one of claims 1 to 3, Features: The following steps are involved: Step 1, adding polyvinyl alcohol to water and mixing evenly, then adding modified polyvinyl alcohol and mixing evenly to obtain a mixed solution; Step 2, add 1 / 3-1 / 2 of the formula amount of n-butyraldehyde to the above mixed solution and mix evenly, heat to 80-90°C, add 1 / 3-1 / 2 of the formula amount of acid, keep 80-90°C to continue the reaction for 2-4h, and cool to 25-35°C; Step 3, continue to add dipentaerythritol and the remaining n-butyraldehyde, heat to 65-80°C, add the remaining acid, continue the reaction for 1-2h, cool to room temperature after the reaction is completed, filter the precipitate, wash with water, soak it in 5-10wt% sodium hydroxide aqueous solution for 30-60min, then wash with water and dry to obtain a high-efficiency polyvinyl butyral resin.