A blended membrane for sulfur-iodine flow battery, preparation method and use

By using a blended membrane prepared by blending modified intrinsic microporous polymer materials and perfluorosulfonic acid resin in sulfur-iodine flow batteries, the problem of capacity attenuation caused by cross-contamination of polysulfides and polyiodides is solved, and the battery life is improved. Coulombic efficiency and stability of the battery extend cycle life.

CN117417610BActive Publication Date: 2024-10-18NANJING TECH UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311148012.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-06
Publication Date
2024-10-18
Estimated Expiration
2043-09-06

AI Technical Summary

Technical Problem

Existing sulfur-iodine flow batteries suffer from rapid capacity attenuation due to cross-contamination of polysulfides and polyiodides during long-term operation, and their cycle life is short, so they lack effective long-life solutions.

Method used

Perfluorosulfonic acid is used as the base membrane, and modified inherently microporous polymer materials (PIMs) are dispersed in it. By blending cPIM-1 with a cyano group modified into a carboxyl group and a perfluorosulfonic acid resin, a polymer with improved performance is prepared. Mechanically strong and ion-selective blend membranes for sulfur-iodine flow batteries.

Benefits of technology

The Coulombic efficiency and overall performance of the sulfur-iodine flow battery are significantly improved, the cycle life of the battery is extended, and the stability and ion selectivity of the membrane are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117417610B_ABST
    Figure CN117417610B_ABST
Patent Text Reader

Abstract

The present invention discloses the synthesis and application of a functionally modified rigid skeleton polymer. The modification method described in the present invention is to hydrophobize a microporous polymer with a rigid skeleton structure, and modify the cyano group on its surface into a hydrophilic group carboxyl group, thereby preparing a new hydrophilic microporous polymer with a rigid skeleton. A perfluorosulfonic acid polymer with high proton conductivity is selected as a base membrane, and is blended with the above-mentioned modified microporous polymer to form a membrane, thereby successfully preparing a perfluorosulfonic acid blended membrane with a supporting skeleton structure. On the one hand, the carboxyl group on the surface of the microporous polymer can form a hydrogen bond network with the sulfonic acid group in the perfluorosulfonic acid to promote the transmission of ions; on the other hand, the inherent micropores of the microporous polymer itself can play a certain role in ion screening, and the twisted helical skeleton polymer can fix the chains in the polymer by winding and binding to prevent them from moving, thereby improving the stability of the membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a blended membrane for a sulfur-iodine liquid flow battery, a preparation method and application thereof, and belongs to the technical field of sulfur-iodine liquid flow batteries. Background Art

[0002] Since the existing clean energy sources such as solar energy and wind energy are intermittent and are limited by time and space to a certain extent, large-scale energy storage systems of grid specifications are needed to smooth out the peak. At present, aqueous redox flow batteries (ARFBs) are a promising energy storage technology due to their high safety and flexible design (energy and power are independent of each other). However, the high chemical cost (all-vanadium flow battery), low energy density (organic system flow battery) and poor long-term stability (zinc-based flow battery) have limited the development of ARFBs.

[0003] Sulfur-iodine flow battery is a large-scale energy storage RFB system with great development potential. The polysulfides and polyiodides that make up its positive and negative electrolytes have high solubility in water, which makes the sulfur-iodine flow battery have a high energy density, and the low chemical cost is also conducive to its large-scale production. However, during long-term operation, polysulfides and polyiodides are prone to cross-contamination, which causes their capacity to decay rapidly, making the cycle life of sulfur-iodine flow batteries short. For example, in the first report on sulfur-iodine flow batteries, two perfluorosulfonic acid membranes (i.e., Nafion117 / Nafion115) were used as battery membranes, and only 50 cycles were run at 80% state of charge (SOC). Therefore, an effective method to achieve long-life polysulfide redox flow batteries is still being sought. Summary of the invention

[0004] The first object of the present invention is to provide a blended membrane for sulfur-iodine flow battery, which uses perfluorosulfonic acid as a base membrane and disperses modified intrinsic microporous polymer materials (PIMs) therein, wherein the PIMs material is cPIM-1 obtained by acidifying PIM-1 with cyano groups and modifying the cyano groups to carboxyl groups.

[0005] A blended membrane for sulfur-iodine liquid flow battery comprises a matrix resin and a surface carboxylated intrinsic microporous polymer material (PIMs) dispersed in the matrix resin.

[0006] The matrix resin is perfluorosulfonic acid resin.

[0007] The surface carboxylation inherent microporous polymer material is obtained by polymerizing TTSBI and then performing a carboxylation treatment.

[0008] The weight ratio of the intrinsic microporous polymer material in the matrix resin is 0.1-50%, preferably 1-5%.

[0009] The thickness of the blended film is 10-200 μm, preferably 120-200 μm.

[0010] A method for preparing a blended membrane for a flow battery comprises the following steps:

[0011] The inherent microporous polymer material is mixed with the perfluorosulfonic acid resin solution in proportion, stirred evenly and degassed to obtain a blended solution, the blended solution is cast on a substrate, and a blended film is obtained after drying.

[0012] The preparation method of the inherent microporous polymer material comprises the following steps: adding TTSBI and tetrafluoroterephthalic acid into a solvent, then adding potassium carbonate for reaction, and washing, recrystallizing and drying the product to obtain the product.

[0013] The weight ratio of TTSBI, tetrafluoroterephthalic acid and potassium carbonate is 5:2-5:2-6, and the solvent used is DMF.

[0014] The reaction conditions are 60-140°C for 10-40h.

[0015] The washing process uses water.

[0016] The solvents used are ethanol, perfluorosulfonic acid solution, etc.

[0017] The drying process first adopts normal pressure and then reduced pressure, the drying temperature is 25-120°C, and 100°C is most preferred; the drying time is 1-48h, and 24h is most preferred.

[0018] Application of the above blended membrane in liquid flow batteries.

[0019] The liquid flow battery is an alkaline sulfur-iodine liquid flow battery with a positive electrode of polyiodide and a negative electrode of polysulfide.

[0020] PIMs materials are used to improve the mechanical strength of blend films, inhibit swelling rate and improve Coulomb efficiency.

[0021] Beneficial Effects

[0022] The present invention blends a cPIMs material with micropores with a perfluorosulfonic acid solution to prepare a membrane. The performance of the resulting blended membrane includes optimizing the ion selectivity of the diaphragm and improving the stability, thereby developing a new generation of high-performance PEM for the application of the RFB system. In the present invention, by adding a PIMs material with a hydrophilic group to a polymer substrate, the application of the blended membrane in the field of redox flow batteries including all-vanadium flow batteries, zinc-iron flow batteries, sulfur-iodine flow batteries, etc. can be improved. By introducing the PIMs material, the ion screening effect of its inherent micropores can effectively inhibit the shuttling of polysulfides and polyiodides, thereby greatly enhancing the ion selectivity of the membrane, thereby increasing the Coulombic efficiency (CE) of the sulfur-iodine flow battery and improving the overall performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 a) Schematic diagram of the synthesis of cPIM-1 b) Infrared image of cPIM-1 c) BET test spectrum of cPIM-1 d) Miscibility of PIM-1 (left) and cPIM-1 (right) in perfluorosulfonic acid resin solution

[0024] Figure 2 This is the electron microscope image of the cross section of Nafion / cPIM-X (X = 0, 1, 2, 3, 4, 5%)

[0025] Figure 3 a) Proton conductivity, b) Water absorption and swelling rate, c) Tensile strength and d) Thermogravimetry of Nafion / cPIM-X (X = 0, 1, 2, 3, 4, 5%)

[0026] Figure 4 Performance diagram of all-vanadium liquid flow battery a) Schematic diagram of sulfur-iodine liquid flow battery, b) CE, c) VE, d) EE at 10-50 mA cm -2 At current density, SOC is set to 50%

[0027] Figure 5 The following are the cycle test diagrams of sulfur-iodine flow battery: a) CE, EE, b) capacity decay diagram (current density is 20 mA cm -2 , SOC is set to 80%)

[0028] Figure 6 I is the ion permeation diagram of polysulfide and polyiodide a)I 3 - Penetration testing, b)S 2 2- Penetration Testing DETAILED DESCRIPTION

[0029] The present invention discloses the synthesis and application of a functionally modified rigid skeleton polymer. The modification method described in the present invention is to hydrophobize a microporous polymer with a rigid skeleton structure, modify the cyano group on its surface into a hydrophilic group carboxyl group, and prepare a new hydrophilic microporous polymer with a rigid skeleton. A perfluorosulfonic acid polymer with high proton conductivity is selected as a base membrane, and is blended with the above-mentioned modified microporous polymer to form a membrane, thereby successfully preparing a perfluorosulfonic acid blended membrane with a supporting skeleton structure. On the one hand, the carboxyl group on the surface of the microporous polymer can form a hydrogen bond network with the sulfonic acid group in the perfluorosulfonic acid to promote the transmission of ions; on the other hand, the inherent micropores of the microporous polymer itself can play a certain role in ion screening, and the twisted helical skeleton polymer can fix the chain in the polymer by winding and restraining it to prevent it from moving, thereby improving the stability of the membrane. This polymer-polymer blending method provides a strategy to improve the stability of the diaphragm, and it is applied to sulfur-iodine liquid flow batteries to test the battery performance.

[0030] The PIMs material used in the following examples is a rigid twisted skeleton material, and the twisted conformation of the inherent microporous polymer molecular chain prevents the polymer chains from being densely packed in space, thereby forming inherent micropores. The inherent micropores can form an ion screening layer to hinder the penetration of ions. On the other hand, the carboxyl groups on the surface of the inherent microporous polymer and the sulfonic acid groups on the surface of the commonly used perfluorosulfonic acid can form a hydrogen bond network to promote the transmission of ions, and the twisted skeleton structure of the PIMs material itself can restrain the movement of the polymer chain, thereby improving the stability of the polymer.

[0031] A hydrophilically modified intrinsic microporous polymer is selected and mixed with a perfluorosulfonic acid solution in a certain ratio to prepare a proton exchange membrane with excellent performance. The present invention can be used to prepare a proton exchange membrane with a reinforced skeleton, and can be applied to the field of redox flow batteries including all-vanadium flow batteries, sulfur-iodine flow batteries, zinc-iron flow batteries, etc.

[0032] The sieving type PIMs used in the present invention are selected from cyano PIM (PIM-1) and modified into cPIM (cPIM-1) by acidification.

[0033] For the material of the present invention, fluorine-containing polymer is mainly used as the organic polymer phase; the hydrophilic intrinsic microporous polymer used in the blending can be selected from the hydrophobic intrinsic microporous polymer modified cPIM with carboxyl functional group (cPIM-1).

[0034] Example 1 Preparation of cPIM-1

[0035] Synthesis of cPIM-1: 5.105 g of 5,5',6,6'-tetrahydroxy-3,3,3',3'-tetramethyl-1,1'-spirobisindane (TTSBI monomer a) and 3.57 g of tetrafluoroterephthalic acid (monomer b) were added to a 250 mL three-necked flask, and then 100 mL of DMF solution was added and mixed evenly. After the mixture was heated to 70°C, 4.228 g of potassium carbonate was added and the reaction was continued at 70°C for 24 hours. After the reaction was completed and cooled to room temperature, it was filtered, and the filtrate was placed in a 60°C oven for drying, and then water was added thereto for washing. After the filter cake was filtered, it was vacuum dried at 120°C for 24 hours. The water washing step was repeated 2-3 times to obtain cPIM-1 powder. The synthesis reaction principle is as follows Figure 1 As shown. This reaction is a nucleophilic aromatic substitution reaction between two monomers to obtain Figure 1 The solubility of the cPIM-1 synthesized by this method in alcohol substances (such as perfluorosulfonic acid resin solution) is much higher than that of PIM-1 such as Figure 1 As shown in b.

[0036] Example 2 Preparation of Nafion / cPIM blend membrane

[0037] Dissolve cPIM-1 powder in 10mL of perfluorosulfonic acid resin dispersion. The solution used was purchased from Dongyue Future Hydrogen Energy. The solid content of the solution was 5.28. Then, according to the mass of each membrane, a certain volume of solution was weighed and mixed with the pure perfluorosulfonic acid resin solution. The new mixture was stirred for 24 hours and ultrasonically treated to form a mixed solution of Nafion / cPIM after being fully uniform. The prepared mixture was poured on a glass culture dish, first placed in a vacuum oven at 100°C and dried at normal pressure for 2 hours, and then vacuumed and dried for another 24 hours. The prepared blended membrane is represented by Nafion / cPIM-x, where x represents the mass ratio of cPIM-1 and the entire membrane.

[0038] In this embodiment, carboxylated TTSBI is used to prepare the membrane. If uncarboxylated TTSBI is used directly, the miscibility is very poor (e.g. Figure 1 As shown in the d area, the dispersion in the resin solution cannot be completed, and the film preparation and battery performance testing cannot be continued.

[0039] Test Method

[0040] Swelling rate and water absorption

[0041] The SR (swelling rate) and WU (water absorption rate) of the membrane are obtained by the following two equations:

[0042]

[0043]

[0044] Where d and W are the diameter and mass of the membrane in wet and dry states, respectively.

[0045] Mechanical properties

[0046] At a pulling speed of 5 mm min -1 The mechanical properties of the membrane were obtained on a universal testing machine. The samples were cut into 35mm×10mm strips and the water on the wet membrane surface was wiped off before testing. In order to reduce the test error, three samples were tested for each membrane and the obtained data were averaged. The tensile strength of the film sample was calculated as follows:

[0047]

[0048] In the formula, F Max is the maximum tension; W and D are the width and thickness of the sample film, respectively.

[0049] Proton transfer rate

[0050] The proton transfer rate of the membrane was measured by AC impedance spectroscopy on an electrochemical workstation (Solartron analytical 1470E+1260A). The sample was sandwiched between two round titanium sheets, which were fixed with button cell clips. The test frequency was 10 3 Up to 10 6 The AC amplitude is 5mV. The proton transfer rate of the membrane is measured using the latest method of Professor Li's team, and the calculation formula is as follows:

[0051]

[0052] Where σ is the proton transfer rate of the membrane. L is the thickness of the sample. R is the impedance of the membrane. A is the effective area of ​​the membrane, that is, the area of ​​the titanium sheet.

[0053] The membrane surface resistance can be calculated by the following formula:

[0054] R A =R×A

[0055] R A is the membrane surface resistance.

[0056] Thermogravimetric testing

[0057] The thermochemical stability of the polymer was evaluated using a thermogravimetric analyzer (TGA, NETZSCH STA209F1). The heating temperature was set at 10 °C min-1, the temperature range was set at 25-800 °C, and the entire test process was carried out under a nitrogen atmosphere.

[0058] Ion permeation rate and ion selectivity

[0059] The effective area is 0.78cm 2 The H-type diffusion cell was tested. One side of the diffusion cell was filled with 10 mL of 3M K 2 S 2 / 1.0M KOH solution or 4M KI solution, and the other side of the diffusion cell is filled with the same volume of aqueous solution, and magnetic stirring is used to reduce concentration polarization during the test. Samples are taken from the aqueous solution every 12 hours, and the absorbance is measured at 300nm using a UV-visible spectrophotometer. The standard absorbance / concentration curve is used to determine S 2 2- or I 3 - The penetration rate of polysulfide and polyiodide can be calculated by the following formula:

[0060]

[0061]

[0062] Where V B 3M K 2 S 2 / 1.0M KOH solution volume, 10ml in this experiment; C B (t) is 3M K at time t 2 S 2 / 1.0M KOH solution S 2 2- The concentration of ions; C A 3M K 2 S 2 / S in 1.0M KOH solution 2 2- Concentration, when the test time is not too long, can be considered as a constant to simplify the calculation; A and L are the effective membrane area and membrane thickness respectively; P is S 2 2- penetration rate.

[0063] Ion selectivity is defined as the ratio of proton transfer rate to S 2 2- The ratio of the permeability rates is calculated as follows:

[0064]

[0065] Basic Characterization of Membranes

[0066] Figure 3 This is a photo of a pure diaphragm cross section.

[0067] Single cell performance

[0068] The performance of PSIB was tested using a homemade sulfur-iodine flow battery system consisting of a membrane (with an effective distance of 10.5 cm 2 ), a carbon felt electrode, a carbon felt electrode, two graphite plate current collectors and a pair of shells. Membrane separator negative electrode electrolyte (10ml 3M K 2 S 2 / 1.0M KOH) and cathode electrolyte (10ml 4M KI) and sandwiched between two electrodes. For the charge and discharge tests, the charge process was controlled by the charge capacity (SOC was set to 50%) and the cut-off voltage (set to 1.9V), and the discharge process was controlled by the cut-off voltage, which was set to 0.2V. The current densities tested were 10, 20, 30, 40, and 50mA cm -2 For the cycling test, the constant current density was 20 mA cm -2 The test was carried out at the same cut-off voltage. In order to make the test environment more harsh, the SOC was increased to 80%. During the test, nitrogen protection was used. The coulomb efficiency (CE), voltage efficiency (VE) and energy efficiency (EE) of the battery were calculated by the following formula:

[0069]

[0070]

[0071]

[0072] Among them C d and C c are the discharge capacity and the charge capacity respectively; E d and E c They are discharge energy and charge energy respectively.

[0073] The PSIB performance of Nafion / cPIM-X blend membranes was evaluated (at 20-100 mA cm -2 under a series of current densities). Figure 5 As shown, the cell performance (CE) of Nafion membrane can be significantly improved by loading cPIM-1. This result shows that incorporating porous PIMs materials into polymers can effectively improve battery performance.

[0074] I 3 - / S 2 2- Penetration Testing

[0075] like Figure 6 As shown, the membrane was subjected to 3 - / S 2 2-Permeability measurements were performed to evaluate ion selectivity. All hybrid membranes with cPIM-1 added showed lower I 3 - / S 2 2 Ion permeability. Due to the modulation of cPIM-1 on Nafion polymer chains, I 3 - / S 2 2- The permeation rate of ions decreases with the increase of cPIM-1 loading. 3 - / S 2 2- The ion permeability was reduced to 2.54×10 -7 cm -2 h -1 and 1.46×10 -6 cm -2 h -1 , much lower than the original Nafion (I 3 - / S 2 2- The permeability is 2.13×10 -6 cm -2 h -1 and 7.69×10 -6 cm -2 h -1 ), the result is as follows Figure 6 In addition, electrochemical impedance spectroscopy was used to further study the K + After adding cPIM-1, as the number of sulfonic acid groups in the membrane decreases, the proton conductivity of the membrane decreases (e.g. Figure 3 a). It is generally believed that the ion selectivity of a membrane is the ratio of conductivity to permeability. After adding cPIM-1, the ion selectivity of the blended membrane tends to increase.

Claims

1. A blended membrane for sulfur-iodine flow battery, characterized in that: The invention comprises a matrix resin and a surface carboxyl-grouped intrinsic microporous polymer material dispersed in the matrix resin; The matrix resin is perfluorosulfonic acid resin; The weight percentage of the surface carboxylated intrinsic microporous polymer material in the matrix resin is 1-5%; the thickness of the blended film is 10-200 μm; The preparation method of the surface carboxylated intrinsic microporous polymer material comprises the following steps: adding 5,5',6,6'-tetrahydroxy-3,3,3',3'-tetramethyl-1,1'-spirobisindane and tetrafluoroterephthalic acid to DMF, then adding potassium carbonate to react, washing, recrystallizing and drying the product to obtain; The weight ratio of 5,5',6,6'-tetrahydroxy-3,3,3',3'-tetramethyl-1,1'-spirobisindane, tetrafluoroterephthalic acid and potassium carbonate is 5:2-5:2-6; The reaction conditions are 60-140°C for 10-40h; Water is used in the washing process, and chloroform, methanol or a mixture of the two is used in the recrystallization process.

2. The blended membrane for sulfur-iodine flow battery according to claim 1, characterized in that: The thickness of the blended film is 120-200 μm.

3. The method for preparing the blended membrane for sulfur-iodine flow battery according to claim 1, characterized in that: The steps include: The inherent microporous polymer material with surface carboxylation is mixed with the perfluorosulfonic acid resin solution in proportion, stirred evenly and degassed to obtain a blended solution, the blended solution is cast on a substrate, and dried to obtain a blended film.

4. The preparation method according to claim 3, characterized in that: The drying process first uses normal pressure and then reduced pressure, the drying temperature is 25-120°C and the drying time is 1-48h.

5. Use of the blended membrane according to claim 1 in a liquid flow battery.

6. The use according to claim 5, characterized in that: The liquid flow battery is an alkaline sulfur-iodine liquid flow battery with a positive electrode of polyiodide and a negative electrode of polysulfide.

Citation Information

Patent Citations

  • Sulfydryl-functionalized microporous polymer as well as preparation and application of sulfydryl-functionalized polymer of intrinsic microporosity (PIM-1)

    CN112521596A

  • Low-molecular-weight intrinsic microporous polymer, preparation method, ultrathin organic solvent nanofiltration film and preparation method of ultrathin organic solvent nanofiltration film

    CN112851690A