A method for recovering lithium from waste ternary lithium-ion battery positive electrode material
By using a combined method of 4,4',4''-s-triazine-2,4,6-triyl-trityl-tribenzoic acid and organic base in waste ternary lithium-ion battery cathode materials, leaching and solvothermal reaction, solving the problems of low lithium recovery rate and purity, achieving more efficient lithium ion recovery and higher purity lithium carbonate precipitation.
Patent Information
- Application Number
- CN202311750378.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-19
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-12-19
AI Technical Summary
In the existing technology, the comprehensive recovery rate and purity of lithium in waste lithium-ion batteries are low, especially in ternary cathode materials, which makes it difficult to effectively recover and purify lithium elements.
A mixed solvent of 4,4',4''-s-triazine-2,4,6-triyl-tribenzoic acid dissolved in N,N-dimethylformamide and methanol was used for leaching treatment, combined with solvothermal The reaction and organic base adjust the pH value, and improve the recovery rate and purity of lithium ions by generating MOF intermediate products and carbonate precipitation reactions.
The recovery rate of lithium and the purity of the recovered products are significantly improved. Compared with the existing technology, more efficient lithium ion recovery and higher-purity lithium carbonate precipitation are achieved.
Smart Images

Figure CN117512342B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of recycling and regenerating waste lithium-ion batteries, and in particular relates to a method for recycling lithium from positive electrode materials of waste ternary lithium-ion batteries. Background Art
[0002] [Lithium-ion batteries are widely used in electronic products such as portable devices and electric vehicles due to their high operating voltage, light weight, no memory effect, and long cycle life. In addition, with the development of electric vehicles, lithium-ion batteries with ternary positive electrodes are widely used due to their high energy density and good stability. Waste lithium-ion batteries contain valuable metals such as nickel, cobalt, manganese (or aluminum), and lithium. How to reasonably handle and recycle waste lithium-ion batteries is an urgent problem to be solved.
[0003] At present, the recycling technology of waste lithium-ion batteries mainly has the problem that the comprehensive recovery rate of lithium is still low and the purity of the recovered Li2CO3 is low. For example, the prior art CN113862476A adopts a recycling method of pre-extracting lithium from the electrode active material and then recovering valuable metal elements such as nickel, cobalt and manganese. Specifically, the prior art performs hydrothermal reaction treatment on the electrode active material after alkali washing and impurity removal, enriches lithium in the leachate after hydrothermal treatment, and then purifies and removes impurities and precipitates lithium to recover lithium. However, the comprehensive recovery rate of lithium in this method is only 85%. Summary of the invention
[0004] The purpose of the present invention is to provide a method for recovering lithium from waste ternary lithium-ion battery positive electrode materials to solve the existing technical problems of low comprehensive lithium recovery rate and purity.
[0005] The method for recovering lithium from waste ternary lithium-ion battery positive electrode materials of the present invention comprises the following steps in sequence:
[0006] (1) Pre-treating waste ternary lithium-ion batteries to obtain positive electrode material powder;
[0007] (2) dissolving 4,4',4''-s-triazine-2,4,6-triyl-tribenzoic acid in a mixed solvent of N,N-dimethylformamide and methanol to obtain a clear solution, adding the positive electrode material powder to the clear solution, heating and stirring for 2-6 hours to obtain a leachate;
[0008] (3) transferring the leachate to a high-pressure reactor lined with corrosion-resistant material, and performing a solvent thermal reaction at 90-180° C. for 12-24 hours. After the reaction is completed, solid-liquid separation is performed to obtain a lithium-rich solution;
[0009] (4) adjusting the pH value of the lithium-rich solution to 9-11 using an organic base, filtering out the residue, and obtaining a lithium-rich filtrate;
[0010] (5) Using carbonate or bicarbonate to carry out precipitation reaction on the lithium-rich filtrate, heating and stirring to obtain lithium carbonate precipitate.
[0011] Furthermore, the pretreatment in step (1) includes decomposing and splitting the battery to obtain a positive electrode sheet, peeling off the positive electrode sheet to obtain a positive electrode material, and crushing and calcining the positive electrode material to obtain the positive electrode material powder.
[0012] Furthermore, in the clear solution of step (2), the concentration of 4,4',4''-s-triazine-2,4,6-triyl-tribenzoic acid is 0.5-1 mol / L, and the volume ratio of N,N-dimethylformamide to methanol is 1:(1-1.5).
[0013] Furthermore, in step (2), the positive electrode material powder is added to the clarified solution at a solid-liquid ratio of 5-50 g / L.
[0014] Furthermore, the heating temperature in step (2) is 40-60°C.
[0015] Furthermore, the temperature of the solvent thermal reaction in step (3) is 140-180° C., and the reaction time is 12-18 hours.
[0016] Furthermore, the solid-liquid separation in step (3) includes filtration or centrifugation.
[0017] Furthermore, the organic base in step (4) is triethylamine and / or triethylenediamine.
[0018] Furthermore, the carbonate or bicarbonate in step (5) is a carbonate or bicarbonate of ammonium, sodium or potassium.
[0019] Furthermore, it is characterized in that the heating temperature in step (5) is 40-60°C.
[0020] Beneficial effects of the present invention:
[0021] (1) The present invention uses a DMF / methanol solution of 4,4',4''-s-triazine-2,4,6-triyl-tribenzoic acid as a leaching reagent for the positive electrode material powder. The central triazine ring and the three benzene rings form a delocalized large π bond. Compared with 1,3,5-benzenetricarboxylic acid, it has better selectivity for metal ions in the ternary positive electrode material, can promote the leaching of metal ions such as Li, Ni, Co, Mn / Al, etc., improve the ion leaching rate, and thus improve the metal recovery rate.
[0022] (2) During the solvothermal reaction, 4,4',4''-s-triazine-2,4,6-triyl-tribenzoic acid reacts efficiently with high-valent Ni, Co, and Mn / Al ions to generate ternary MOF intermediates. Among them, the three carboxylic acid groups in the phenyltriazine tricarboxylic acid organic ligands can coordinate with the Ni, Co, and Mn ions or Ni, Co, and Al ions in the ternary metals, further inducing the enrichment of lithium ions in the solution. While improving the lithium ion recovery rate, the purity of the recovered lithium carbonate product can be further improved.
[0023] (3) The liquid phase in the lithium-rich solution of the present invention is an organic phase. The use of organic bases such as triethylamine and / or triethylenediamine to adjust the pH value of the lithium-rich solution can achieve a good compatibility and efficiently remove impurities from the lithium-rich solution. In addition, the selection of the above-mentioned organic bases can avoid the introduction of other metal ions in this step, thereby improving the purity of the recovered product.
[0024] (4) The present invention uses 4,4',4''-s-triazine-2,4,6-triyl-tribenzoic acid in the leaching process and the dissolution heat step, and uses an organic base to remove impurities from the lithium-rich solution obtained by the solvent thermal reaction. Compared with the prior art, the lithium recovery rate can be effectively improved and the purity of the recovered product can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The figure is a flow chart of an embodiment of the present invention.
[0026] Figure 2 This is the XRD pattern of lithium carbonate obtained in Example 1. DETAILED DESCRIPTION
[0027] The present invention is further described below with reference to examples and comparative examples.
[0028] Example 1
[0029] This embodiment includes the following steps:
[0030] Waste nickel-cobalt-manganese ternary lithium-ion batteries are decomposed and split to obtain positive electrode sheets, positive electrode materials are peeled off from the positive electrode sheets, and the positive electrode materials are crushed and calcined to obtain positive electrode material powder; 4,4',4''-s-triazine-2,4,6-triyl-tribenzoic acid is dissolved in a mixed solvent of N,N-dimethylformamide and methanol to obtain a clear solution, wherein the molar concentration of 4,4',4''-s-triazine-2,4,6-triyl-tribenzoic acid in the clear solution is 1 mol / L, the volume ratio of N,N-dimethylformamide to methanol is 1:1, and the mixture is stirred at 50 ℃ for 2 hours. g / L solid-to-liquid ratio, adding the positive electrode material powder to the clarified solution, heating to 60°C and stirring for 2h to obtain a leachate; transferring the leachate to a polytetrafluoroethylene-lined high-pressure reactor to perform a solvent thermal reaction, the temperature of the solvent thermal reaction is 180°C, the reaction time is 12h, after the reaction is completed, filtering to obtain a lithium-rich solution; using triethylamine to adjust the pH value of the lithium-rich solution to 10, filtering out the residue to obtain a lithium-rich filtrate; finally, using sodium carbonate to perform a precipitation reaction on the lithium-rich filtrate, heating to 60°C and stirring, and collecting to obtain a lithium carbonate precipitate.
[0031] Example 2
[0032] This embodiment includes the following steps:
[0033] Waste nickel-cobalt-manganese ternary lithium-ion batteries are decomposed and split to obtain positive electrode sheets, positive electrode materials are peeled off from the positive electrode sheets, and the positive electrode materials are crushed and calcined to obtain positive electrode material powder; 4,4',4''-s-triazine-2,4,6-triyl-tribenzoic acid is dissolved in a mixed solvent of N,N-dimethylformamide and methanol to obtain a clear solution, wherein the molar concentration of 4,4',4''-s-triazine-2,4,6-triyl-tribenzoic acid in the clear solution is 0.5 mol / L, the volume ratio of N,N-dimethylformamide to methanol is 1:1.5, and the mixture is stirred at 50 ℃ for 1 h. g / L solid-liquid ratio, adding the positive electrode material powder to the clarified solution, heating to 40°C and stirring for 6 hours to obtain a leachate; transferring the leachate to a polytetrafluoroethylene-lined high-pressure reactor to perform a solvent thermal reaction, the temperature of the solvent thermal reaction is 90°C, the reaction time is 24 hours, after the reaction is completed, filtering to obtain a lithium-rich solution; using triethylamine to adjust the pH value of the lithium-rich solution to 9, filtering out the residue to obtain a lithium-rich filtrate; finally, using sodium bicarbonate to perform a precipitation reaction on the lithium-rich filtrate, heating to 40°C and stirring, and collecting to obtain lithium carbonate precipitate.
[0034] Example 3
[0035] This embodiment includes the following steps:
[0036] Waste nickel-cobalt-aluminum ternary lithium-ion batteries are decomposed and split to obtain positive electrode sheets, positive electrode materials are peeled off from the positive electrode sheets, and the positive electrode materials are crushed and calcined to obtain positive electrode material powder; 4,4',4''-s-triazine-2,4,6-triyl-tribenzoic acid is dissolved in a mixed solvent of N,N-dimethylformamide and methanol to obtain a clear solution, wherein the molar concentration of 4,4',4''-s-triazine-2,4,6-triyl-tribenzoic acid in the clear solution is 1 mol / L, the volume ratio of N,N-dimethylformamide to methanol is 1:1.5, and the mixture is stirred at 25 ℃ for 24 hours. g / L of solid-liquid ratio, adding the positive electrode material powder to the clarified solution, heating to 40°C and stirring for 6 hours to obtain a leachate; transferring the leachate to a polytetrafluoroethylene-lined high-pressure reactor to perform a solvent thermal reaction, the temperature of the solvent thermal reaction is 140°C, the reaction time is 18 hours, after the reaction is completed, filtering to obtain a lithium-rich solution; using triethylenediamine to adjust the pH value of the lithium-rich solution to 11, filtering out the residue to obtain a lithium-rich filtrate; finally, using sodium carbonate to perform a precipitation reaction on the lithium-rich filtrate, heating to 60°C and stirring, and collecting to obtain a lithium carbonate precipitate.
[0037] Example 4
[0038] This embodiment includes the following steps:
[0039] Waste nickel-cobalt-aluminum ternary lithium-ion batteries are decomposed and split to obtain positive electrode sheets, positive electrode materials are peeled off from the positive electrode sheets, and the positive electrode materials are crushed and calcined to obtain positive electrode material powder; 4,4',4''-s-triazine-2,4,6-triyl-tribenzoic acid is dissolved in a mixed solvent of N,N-dimethylformamide and methanol to obtain a clear solution, wherein the molar concentration of 4,4',4''-s-triazine-2,4,6-triyl-tribenzoic acid in the clear solution is 0.5 mol / L, the volume ratio of N,N-dimethylformamide to methanol is 1:1, and the mixture is stirred at 10 ℃ for 2 hours. g / L solid-liquid ratio, adding the positive electrode material powder to the clarified solution, heating to 60°C and stirring for 4 hours to obtain a leachate; transferring the leachate to a polytetrafluoroethylene-lined high-pressure reactor to perform a solvent thermal reaction, the temperature of the solvent thermal reaction is 100°C, the reaction time is 24 hours, after the reaction is completed, filtering to obtain a lithium-rich solution; using triethylenediamine to adjust the pH value of the lithium-rich solution to 10, filtering out the residue to obtain a lithium-rich filtrate; finally, using sodium bicarbonate to perform a precipitation reaction on the lithium-rich filtrate, heating to 50°C and stirring, and collecting to obtain lithium carbonate precipitate.
[0040] Comparative Example 1
[0041] This comparative example comprises the following steps:
[0042] Waste nickel-cobalt-manganese ternary lithium-ion batteries are decomposed and split to obtain positive electrode sheets, and positive electrode materials are peeled off from the positive electrode sheets. The positive electrode materials are then crushed and calcined to obtain positive electrode material powder; manganese sulfate monohydrate is dissolved in deionized water to obtain a clear solution, wherein the molar concentration of manganese sulfate monohydrate in the clear solution is 1 mol / L, and the positive electrode material powder is added to the clear solution according to a solid-liquid ratio of 50 g / L, heated to 60°C and stirred for 2 hours to obtain a mixed solution; the mixed solution is transferred to a polytetrafluoroethylene-lined high-pressure reactor for hydrothermal reaction at a temperature of 180°C and a reaction time of 12 hours. After the reaction is completed, a lithium-rich solution is obtained by filtering; sodium hydroxide is used to adjust the pH value of the lithium-rich solution to 10, and the residue is filtered to obtain a lithium-rich filtrate; finally, sodium carbonate is used to precipitate the lithium-rich filtrate, heated to 60°C and stirred, and lithium carbonate precipitate is collected.
[0043] Comparative Example 2
[0044] This comparative example comprises the following steps:
[0045] Waste nickel-cobalt-manganese ternary lithium-ion batteries are decomposed and split to obtain positive electrode sheets, positive electrode materials are peeled off from the positive electrode sheets, and the positive electrode materials are crushed and calcined to obtain positive electrode material powder; 1,3,5-benzenetricarboxylic acid is dissolved in a mixed solvent of N,N-dimethylformamide and methanol to obtain a clear solution, wherein the molar concentration of 1,3,5-benzenetricarboxylic acid in the clear solution is 1 mol / L, the volume ratio of N,N-dimethylformamide to methanol is 1:1, and the mixture is stirred at 50 ℃ for 2 hours. g / L solid-to-liquid ratio, adding the positive electrode material powder to the clarified solution, heating to 60°C and stirring for 2h to obtain a leachate; transferring the leachate to a polytetrafluoroethylene-lined high-pressure reactor to perform a solvent thermal reaction, the temperature of the solvent thermal reaction is 180°C, the reaction time is 12h, after the reaction is completed, filtering to obtain a lithium-rich solution; using triethylamine to adjust the pH value of the lithium-rich solution to 10, filtering out the residue to obtain a lithium-rich filtrate; finally, using sodium carbonate to perform a precipitation reaction on the lithium-rich filtrate, heating to 60°C and stirring, and collecting to obtain a lithium carbonate precipitate.
[0046] Lithium recovery rate Lithium carbonate purity Example 1 92.12% 99.67% Example 2 91.85% 99.56% Example 3 92.06% 99.60% Example 4 91.50% 99.53% Comparative Example 1 85.13% 95.27% Comparative Example 2 87.37% 97.51%
Claims
1. A method for recovering lithium from waste ternary lithium-ion battery positive electrode materials, characterized in that: The following steps are included in sequence: (1) pre-treating waste ternary lithium-ion batteries to obtain positive electrode material powder; (2) dissolving 4,4',4"-s-triazine-2,4,6-triyl-tribenzoic acid in a mixed solvent of N,N-dimethylformamide and methanol to obtain a clear solution, adding the positive electrode material powder to the clear solution, heating and stirring for 2-6 hours to obtain a leachate; (3) transferring the leachate to a high-pressure reactor lined with corrosion-resistant material, performing a solvent thermal reaction at 90-180° C. for 12-24 hours. After the reaction is completed, solid-liquid separation is performed to obtain a lithium-rich solution; (4) using an organic base to adjust the pH value of the lithium-rich solution to 9-11, filtering out the residue to obtain a lithium-rich filtrate; (5) using carbonate or bicarbonate to carry out precipitation reaction on the lithium-rich filtrate, heating and stirring to obtain lithium carbonate precipitate; In the clear solution of step (2), the concentration of 4,4',4"-s-triazine-2,4,6-triyl-tribenzoic acid is 0.5-1 mol / L, and the volume ratio of N,N-dimethylformamide to methanol is 1:(1-1.5); In step (2), the positive electrode material powder is added to the clear solution at a solid-to-liquid ratio of 5-50 g / L; The organic base described in step (4) is triethylamine and / or triethylenediamine.
2. The method according to claim 1, characterized in that The pretreatment in step (1) includes decomposing and splitting the battery to obtain a positive electrode sheet, peeling off the positive electrode sheet to obtain a positive electrode material, and then crushing and calcining the positive electrode material to obtain the positive electrode material powder.
3. The method according to claim 1, characterized in that The heating temperature in step (2) is 40-60°C.
4. The method according to claim 1, characterized in that The temperature of the solvent thermal reaction in step (3) is 140-180° C., and the reaction time is 12-18 hours.
5. The method according to claim 1, characterized in that The solid-liquid separation in step (3) includes filtration or centrifugation.
6. The method according to claim 1, characterized in that The carbonate or bicarbonate described in step (5) is a carbonate or bicarbonate of ammonium, sodium or potassium.
7. The method according to claim 1, characterized in that The heating temperature described in step (5) is 40-60°C.