A method for extracting vanadium and dephosphorizing vanadium from molten iron containing vanadium

Through multiple circulation enrichment processes in the converter, vanadium and phosphorus are enriched into different mineral phases respectively, which solves the problems of low vanadium slag quality and waste of vanadium resources in the existing technology, realizes efficient vanadium resource recovery and steel slag utilization, and improves Improve production efficiency and economic benefits.

CN117512362BActive Publication Date: 2024-10-01YANCHENG LIANXIN IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311606013.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-29
Publication Date
2024-10-01
Estimated Expiration
2043-11-29

AI Technical Summary

Technical Problem

The existing vanadium extraction process from vanadium-containing molten iron has problems such as low vanadium slag quality, low productivity, tight heat, low metal desulfurization rate, and waste of vanadium resources. In particular, when high-vanadium molten iron is used for converter steelmaking, the vanadium element is lost with the steel slag and cannot be effectively recovered. .

Method used

By implementing multiple circulation enrichment processes in the converter, vanadium and phosphorus elements are enriched into different mineral phases in the steel slag respectively, and technologies such as low gun position, high oxygen supply intensity blowing process and magnetic separation are used to control the content of the slag. Alkalinity and metallic iron content form vanadium iron spinel and dicalcium silicate phases to achieve separation and enrichment of vanadium and phosphorus.

Benefits of technology

It improves the grade of vanadium slag, reduces the consumption of steel materials, achieves effective recovery of vanadium resources and efficient utilization of steel slag, and improves production efficiency and economic benefits.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a method for extracting vanadium and dephosphorizing vanadium from vanadium-containing molten iron, comprising the following steps: S1: blowing a first vanadium-containing molten iron, adding iron oxides in batches during the blowing process, and obtaining a first steel slag after the initial blowing; pouring out the first steel slag for sorting to obtain a first vanadium-containing magnetic substance and a first phosphorus-containing non-magnetic substance; S2: blowing a second vanadium-containing molten iron, adding the first vanadium-containing magnetic substance and / or iron oxides in batches during the blowing process, and obtaining a second steel slag after the initial blowing; pouring out the second steel slag for sorting to obtain a second vanadium-containing magnetic substance and a second phosphorus-containing non-magnetic substance; accordingly, the second vanadium-containing magnetic substance is obtained for blowing a third vanadium-containing molten iron, until SN, SN is blowing an N-th vanadium-containing molten iron, adding an N-1th vanadium-containing magnetic substance and / or iron oxides in batches during the blowing process, and obtaining an N-th steel slag after the initial blowing; pouring out the N-th steel slag for sorting to obtain an N-th vanadium-containing magnetic substance and an N-th phosphorus-containing non-magnetic substance; N≥2, and the vanadium extraction rate of the method can reach more than 90%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steelmaking with vanadium-containing molten iron, and in particular to a method for extracting vanadium and dephosphorizing vanadium from vanadium-containing molten iron. Background Art

[0002] At present, hot metal with a relatively high vanadium content (0.15-0.4%) generally adopts a double process, that is, first vanadium slag is blown in a vanadium blowing furnace, and then semi-steel is dephosphorized and steel-made in another converter. However, the converter double-linked vanadium extraction process has certain disadvantages. The vanadium slag blown in the vanadium blowing converter is acidic slag. Under the condition of semi-steel temperature (1370-1420℃), even if the TFe in the vanadium slag reaches 28%, the viscosity of the vanadium slag is still very large, resulting in the MFe content in the slag reaching more than 11%; the productivity of steelmaking in the converter workshop is low, and the semi-steel turnover requires a certain amount of time, which prolongs the smelting cycle; when using semi-steel to make steel, the heat of converter smelting is tight and cannot handle a considerable amount of scrap steel; about 10% of the residual vanadium in the semi-steel is lost with the steel slag after semi-steel steelmaking, and a very small part is lost with the semi-steel slag; due to the small amount of semi-steel steelmaking slag, the metal desulfurization rate is low. The converter single slag method also has disadvantages: the quality of vanadium slag is low, the average mass fraction of V205 is less than 10%; the mass fraction of calcium oxide is as high as about 40%, and there is no effective method to extract vanadium pentoxide. Low-vanadium hot metal containing vanadium ≤ 0.15% is generally not used for vanadium extraction, and lime is directly added for steelmaking. The vanadium element in it is oxidized and poured out with the steel slag and discarded.

[0003] For decades, professionals have conducted a lot of research to obtain vanadium resources from steel slag, but so far no process technology that can be put into industrial application has been developed, resulting in a large amount of vanadium resources being wasted along with the steel slag. Summary of the invention

[0004] 1. Technical issues to be solved

[0005] In view of the deficiencies of the prior art, the present invention provides a method for extracting vanadium and dephosphorizing vanadium from vanadium-containing molten iron, which directly enriches vanadium and phosphorus elements into two different mineral phases in slag during converter steelmaking and dephosphorization to produce vanadium slag.

[0006] (II) Technical solution

[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0008] A method for extracting vanadium and dephosphorizing vanadium from vanadium-containing molten iron, comprising the following steps:

[0009] S1. Implement slag-retaining operation. Add scrap steel to the first vanadium-containing molten iron, perform down-gun blowing on the first vanadium-containing molten iron, add iron oxides in batches during the blowing process, and obtain the first steel slag after the initial blowing; pour out the first steel slag, crush it after cooling, and perform sorting to obtain the first vanadium-containing magnetic material and the first phosphorus-containing non-magnetic material;

[0010] S2. Implement slag retention. Add scrap steel to the second vanadium-containing molten iron, perform down-gun blowing on the second vanadium-containing molten iron, add the first vanadium-containing magnetic material and / or iron oxide in batches during the blowing process, and obtain the second steel slag after the initial blowing; pour out the second steel slag, crush it after cooling, and sort it to obtain the second vanadium-containing magnetic material and the second phosphorus-containing non-magnetic material; accordingly, the obtained second vanadium-containing magnetic material is used for the blowing of the third vanadium-containing molten iron, until,

[0011] SN, implement slag retention operation. Add scrap steel to the Nth vanadium-containing molten iron, blow the Nth vanadium-containing molten iron under the gun, add the N-1th vanadium-containing magnetic material and / or iron oxide in batches during the blowing process, and obtain the Nth steel slag after the initial blowing; pour out the Nth steel slag, crush it after cooling, and sort it to obtain the Nth vanadium-containing magnetic material and the Nth phosphorus-containing non-magnetic material;

[0012] Said N≥2.

[0013] Preferably, the basicity of the first steel slag, the second steel slag and the Nth steel slag is 1.0-1.5.

[0014] Preferably, the metallic iron content in the first steel slag, the second steel slag and the Nth steel slag is 4-12% by mass.

[0015] Preferably, if the vanadium content in the Nth vanadium-containing molten iron is 0.15-0.4 mass %, then N=2, and the vanadium pentoxide content in the Nth vanadium-containing magnetic material is ≥15 mass %.

[0016] Preferably, if the vanadium content in the Nth vanadium-containing molten iron is 0.06-0.15 mass %, then 3≤N≤5, and the vanadium pentoxide content of the Nth vanadium-containing magnetic material is ≥8 mass %.

[0017] Preferably, the basicity of the first steel slag, the second steel slag and the Nth steel slag is 1.3-1.5, and the content of metallic iron in the first steel slag, the second steel slag and the Nth steel slag is 5-10% by mass.

[0018] Preferably, the content of MgO in the first steel slag, the second steel slag and the Nth steel slag is 0-5% by mass.

[0019] Preferably, the lower gun blowing adopts a low gun position and high oxygen supply intensity blowing process, the low gun position is 100-200mm lower than the gun position in the early stage of blowing in the conventional process, and the high oxygen supply intensity is ≥3.0m / (min·t); the sorting includes magnetic separation or gravity separation.

[0020] (III) Beneficial effects

[0021] The present invention provides a method for extracting vanadium and dephosphorizing vanadium from molten iron containing vanadium. Compared with the prior art, the method has the following beneficial effects:

[0022] The method for extracting vanadium and dephosphorizing vanadium from vanadium-containing hot metal of the present invention solves a series of problems existing in the high-vanadium hot metal double-linked method and the single slag process. While satisfying the requirements of steelmaking and dephosphorization in a single converter, the slag can be cooled and sorted to produce a vanadium slag product acceptable to the market; after steelmaking in the low-vanadium hot metal converter, the vanadium element is not discarded with the vanadium-containing steel slag, but is enriched through the cyclic iteration of this process to obtain market value. The more times of repeated enrichment iterations through the technical scheme of the present invention, the higher the grade of the vanadium slag obtained by enriching vanadium, and the lower the steel material consumption of the steel plant; the more times of cyclic enrichment iterations of vanadium-containing magnetic separation, the higher the grade of the vanadium slag obtained, and the lower the steel consumption per ton, because when vanadium is not extracted, each furnace must pour out a considerable amount of slag with a high iron content, which cannot be recycled and must be discarded.

[0023] Compared with the double-smelting converter vanadium extraction process, the process of the present invention pours out the vanadium-containing initial slag alkaline slag, firstly, the basicity is low, R1.3-1.5, and secondly, the V2O5 in the alkaline slag has the effect of diluting the slag. Therefore, under the conditions of lower TFe content and lower temperature (1370-1420℃), the slag has better fluidity and lower metallic iron content, which greatly saves metal consumption.

[0024] In addition, after vanadium is extracted from steel slag by sorting, the remainder can be used for other purposes. Therefore, the process method of the present invention solves the problem of steel slag utilization while producing vanadium slag, and has huge economic and social benefits. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] The embodiments of the present application provide a method for extracting vanadium and dephosphorizing vanadium from vanadium-containing molten iron, thereby solving the technical problem of low content of V205 in vanadium slag in existing methods for extracting vanadium and dephosphorizing vanadium from vanadium-containing molten iron.

[0027] The technical solution in the embodiment of the present application is to solve the above technical problems, and the overall idea is as follows:

[0028] The method for extracting vanadium and dephosphorizing vanadium from molten iron containing vanadium of the present invention controls the basicity of the slag at the initial stage of pouring out to 1.3-1.5, which does not affect dephosphorization. P2O5 in the slag is mainly enriched in dicalcium silicate, and V2O5 is mainly distributed in the iron-containing phase. By controlling a certain metallic iron content in the slag, a certain reducing atmosphere can be maintained in the molten slag after the steel slag enters the slag pot. +5 and V +4 Uniformly reduce to V +3, forming vanadium iron spinel with iron oxide. In this way, phosphorus and vanadium enter the dicalcium silicate phase and vanadium iron spinel phase respectively, and the specific gravity of the two differs by about 50%. One is non-magnetic and the other is magnetic. The two are separated by magnetic separation, wind separation and gravity separation.

[0029] The use of low gun position, high oxygen supply intensity, enhanced molten pool stirring, and control of Fe0 content at 9-15% at the end of blowing are beneficial to dephosphorization under low basicity conditions and to vanadium enrichment.

[0030] The vanadium-containing magnetic material prepared in this application is used iteratively as a coolant to enrich and improve V2O5 in converter slag. After two cycles of enrichment with high-vanadium molten iron, the vanadium slag can meet the national standard. After 3-5 cycles of enrichment with low-vanadium molten iron, the vanadium slag acceptable to the market can be achieved. The (FeO) and metallic iron in the magnetic separation are returned to the converter, which not only replaces the cooling and oxidation of iron oxides, but also greatly reduces iron consumption.

[0031] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with specific implementation methods.

[0032] Example 1

[0033] Hot metal composition C V P S Si Temperature, °C content,% 4.4 0.18 0.10 0.015 0.3 1290

[0034] After the slag splashing of the previous furnace is completed, all the slag remains in the furnace. The full slag retention operation is adopted. 120 tons of molten iron and 10 tons of scrap steel are added. The dust removal fan is accelerated to the right speed to carry out the molten iron and scrap steel addition operations: After the molten iron and scrap steel addition operations are completed, the converter furnace is tilted upward to the zero position in the main control room, and "Start main blowing" is clicked. The lower gun is ignited. After the hydrogen gun is ignited successfully, the gun is quickly lowered to a low gun position of 1.1 meters from the nozzle to the gold liquid surface for blowing (the conventional process is 0.8 meters), the oxygen supply intensity is 3.06m / min / t, and the bottom blowing nitrogen intensity is 0.2Nm 3 / t.min control, without adding any slag, the initial slag basicity is controlled at 1.3-1.5, Mg0 content <5%, iron oxide pellets are added in batches during blowing, the addition amount is controlled at 25kg / t, the FeO content is controlled at 9-15%, oxygen is blown for 5 minutes and 30 seconds, the furnace is poured and the slag is discharged, the temperature is 1390℃. The slag discharged is about 6.2t.

[0035] Semi-steel composition: C 3.8%, V 0.021%, P 0.034%. The calculated vanadium extraction rate is 88% and the dephosphorization rate is 66%.

[0036] Vanadium extraction rate = (vanadium content in molten iron before blowing - vanadium content in semi-steel after blowing) / vanadium content in molten iron before blowing × 100%.

[0037] Dephosphorization rate = (phosphorus content in molten iron before blowing - phosphorus content in semi-steel after blowing) / phosphorus content in molten iron before blowing × 100%.

[0038] The main components of vanadium-containing steel slag are: basicity 1.42, P2O5 3.5%, V2O5 4.5%, TFe 8%, MFe 6.2%.

[0039] The poured slag is transported to the slag treatment plant, and after cooling, it is transported to the slag crushing, grinding and separation plant. The slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that per ton of steel, 20 kg of the first vanadium-containing magnetic material containing 7.2% V2O5 and 12.8% V and 40 kg of the first phosphorus-containing non-magnetic material containing V<1% are obtained.

[0040] The steel consumption per ton of steel is 1068kg / t of steel.

[0041] Example 2

[0042] Hot metal composition C V p S Si Temperature, °C content,% 4.1 0.38 0.08 0.012 0.035 1302

[0043] After the slag splashing of the previous furnace is completed, all the slag is left in the furnace. The full slag operation is adopted, and 125t of molten iron + 12t of scrap steel are added. The dust removal fan is accelerated to the right speed, and the molten iron and scrap steel adding operations are carried out: After the molten iron and scrap steel adding operations are completed, the converter furnace is tilted upward to the zero position in the main control room, and "Start main blowing" is clicked. The lower gun is ignited. After the hydrogen gun is ignited successfully, the gun is quickly lowered to the low gun position of 1.2 meters from the nozzle to the gold liquid surface for blowing. The oxygen supply intensity is 3.06m / min / t, and the bottom blowing nitrogen intensity is 0.2Nm 3 / t.min control, without adding any slag, the slag basicity in the early stage is controlled at 1.3-1.5, the MgO content is <5%, the first vanadium-containing magnetic material of Example 1 is added in batches during the blowing process, the addition amount is controlled at 20kg / t and 10kg / t of sintered ore, oxygen is blown for 5 minutes and 50 seconds, the furnace is poured and the slag is discharged, and the temperature is 1400°C. The discharged slag is about 6t.

[0044] Semi-steel composition: C 3.5%, V 0.0304%, P 0.025%, the calculated vanadium extraction rate is 92%, and the dephosphorization rate is 68%.

[0045] The main components of vanadium-containing steel slag are: basicity 1.5, P2O5 3.4%, V2O5 8.5%, TFe 11%, and MFe 9.1%.

[0046] The poured slag is transported to the slag treatment plant, and after cooling, it is transported to the slag crushing, grinding and separation plant. The slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that per ton of steel, 30 kg of the second vanadium-containing magnetic separation product containing V11.0% equivalent to V2O519.6% and 40 kg of the second phosphorus-containing non-magnetic material containing V<1% are obtained.

[0047] The steel consumption per ton of steel is 1067kg / t of steel.

[0048] Example 3

[0049] Hot metal composition C V P S Si Temperature, °C content,% 4.4 0.06 0.088 0.012 0.31 1323

[0050] After the slag splashing of the previous furnace is completed, all the slag is left in the furnace. The full slag operation is adopted. 120 tons of molten iron and 11 tons of scrap steel are added. The dust removal fan is accelerated to the right speed to add molten iron and scrap steel: After the operation of adding molten iron and scrap steel is completed, the converter furnace is tilted upward to the zero position in the main control room, and "Start main blowing" is clicked. The lower gun is ignited. After the hydrogen gun is ignited successfully, the gun is quickly lowered to the low gun position of 1.1 meters from the nozzle to the gold liquid surface for blowing. The oxygen supply intensity is 3.06m / min / t, and the bottom blowing nitrogen intensity is 0.2Nm 3 / t.min control, without adding any slag, the initial slag breakage is controlled at 1.3-1.5, Mg0 content <5%, iron oxide pellets are added in batches during blowing, the amount added is controlled at 35kg / t, oxygen is blown for 5 minutes and 20 seconds, the furnace is poured and the slag is discharged, the temperature is 1383℃. The slag is about 5.4t.

[0051] Semi-steel composition: C 3.8%, V 0.009%, P 0.029%, the calculated vanadium extraction rate is 85%, and the dephosphorization rate is 66%.

[0052] The main components of vanadium-containing steel slag are: basicity 1.45, P2O5 3.1%, V2O5 1.8%, TFe 8%, MFe7.2%.

[0053] The poured slag is transported to the slag treatment plant, and after cooling, it is transported to the slag crushing, grinding and separation plant. The slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that per ton of steel, 20 kg of the first vanadium-containing magnetic material containing 2.1% V and 40 kg of the first phosphorus-containing non-magnetic material containing V<1% are obtained.

[0054] The consumption of one ton of steel is 1064kg / t of steel.

[0055] Example 4

[0056] Hot metal composition C V P S Si Temperature, °C content,% 4.2 0.09 0.09 0.015 0.30 1310

[0057] The smelting steps are the same as those in Example 3, except that 20 kg / t of the first vanadium-containing magnetic separation material and 15 kg / t of oxidized pellets in Example 3 are added in the later stage of the initial blowing, and the slag is poured out after the blowing is completed.

[0058] Semi-steel composition: C 3.8%, V 0.009%, P 0.033%. The calculated vanadium extraction rate is 90% and the dephosphorization rate is 63%.

[0059] The main components of vanadium-containing steel slag are: basicity 1.43, P2O5 3.3%, V2O5 3.9%, TFe 6.5%, and MFe 7.2%.

[0060] The poured slag is transported to the slag treatment plant, and after cooling, it is transported to the slag crushing, grinding and separation plant. The slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that per ton of steel, 2.6% V is obtained, which is equivalent to 4.6% V2O5. 25kg of the second vanadium-containing magnetic material and 40kg of the second phosphorus-containing non-magnetic material containing V<1% are obtained.

[0061] The steel consumption per ton of steel is 1066kg / t of steel.

[0062] Example 5

[0063] Hot metal composition C V P S Si Temperature, °C content,% 4.3 0.06 0.081 0.014 0.34 1301

[0064] The smelting steps are the same as those of Example 3, except that 25 kg / t of the second vanadium-containing magnetic separation material and 10 kg / t of oxidized pellets of Example 4 are added in the later stage of the initial blowing. After the blowing is completed, the slag is poured out.

[0065] Semi-steel composition: C 3.5%, V 0.009%, P 0.032%, the calculated vanadium extraction rate is 85%, and the dephosphorization rate is 60%.

[0066] The main components of vanadium-containing steel slag are: basicity 1.3, P2O5 3.2%, V2O5 5.5%, TFe 6.5%, MFe 7.2%.

[0067] The poured slag is transported to the slag treatment plant, and after cooling, it is transported to the slag crushing, grinding and separation plant. The slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that per ton of steel, 25kg of the third vanadium-containing magnetic material equivalent to V2O5 8% and 40kg of the third phosphorus-containing non-magnetic material containing V<1% are obtained.

[0068] The consumption per ton of steel is 1063kg / t of steel.

[0069] Example 6

[0070] Hot metal composition C V P S Si Temperature, °C content,% 4.3 0.06 0.088 0.011 0.34 1295

[0071] The smelting steps are the same as those in Example 3, except that 25 kg / t of the third vanadium-containing magnetic separation material and 10 kg / t of oxidized pellets of Example 5 are added in the later stage of the initial blowing. After the blowing is completed, the slag is poured out.

[0072] Semi-steel composition: C 3.5%, V 0.0066%, P 0.035%, the calculated vanadium extraction rate is 89% and the dephosphorization rate is 65%.

[0073] The main components of vanadium-containing steel slag are: basicity 1.5, P2O5 3.1%, V2O5 9.5%, TFe 6.5%, and MFe 7.2%.

[0074] The poured slag is transported to the slag treatment plant, and after cooling, it is transported to the slag crushing, grinding and separation plant. The slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that per ton of steel, 25kg of the fourth vanadium-containing magnetic material containing 6.5% V equivalent to 11.6% V2O5 and 40kg of the fourth phosphorus-containing non-magnetic material containing V<1% are obtained.

[0075] The steel consumption per ton of steel is 1065kg / t of steel.

[0076] Comparative Example 1

[0077] Hot metal composition C V P S Si Temperature, °C content,% 4.3 0.07 0.089 0.013 0.32 1305

[0078] After the last furnace is finished, pour out 50% of the slag and leave 50% of the slag. The slag splashing operation is performed to protect the furnace. After splashing, the remaining slag is left in the furnace. Add 20.2t of scrap steel, 110t of molten iron, and 3t of iron sheet. The converter mouth is tilted upward to zero position, and the lower gun is ignited. After the oxygen gun is successfully ignited, constant pressure variable gun position operation is adopted, the oxygen flow rate is 3.6Nm / t / min, the smelting gun position is controlled at 1.2~1.8m, and the oxygen supply stage is 36%. Lime is added in three batches for a total of 5.4t, and the blowing is 14min06s. At the end of smelting, the terminal temperature is 1648℃, the terminal phosphorus is 0.009%, the final slag basicity is 3.3, the final slag TFe is 15%, and V2O5 is 1.3%.

[0079] The steel consumption per ton of steel is 1065kg / t of steel.

[0080] It can be seen from Examples 1 and 2 that after the high-vanadium molten iron is enriched twice by the technical solution of the present invention, the V content of the vanadium slag is 11%, which is converted into 19.6% V2O5.

[0081] It can be seen from Examples 3 to 6 that after three enrichments according to the technical solution of the present invention, the V content of the vanadium slag of low-vanadium molten iron is converted into 8% V2O5, and the V content of the vanadium slag after four enrichments is 6.5%, which is converted into 11.6% V2O5.

[0082] By comparing Examples 1-6 with Comparative Example 1, it can be seen that the vanadium recovery rate of the low-vanadium molten iron treated by the process of the technical solution of the present invention reaches 60-70%, and the steel material consumption is reduced by about 10kg / t steel.

[0083] In Comparative Example 1, the vanadium in the low-vanadium molten iron is lost along with the steel slag.

[0084] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0085] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them; although the present invention is described in detail with reference to the above embodiments, it should be understood by those skilled in the art that the technical solutions described in the above embodiments can still be modified, or some of the technical features can be replaced by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention. Anything not described in detail in the present invention is a well-known technology to those skilled in the art.

Claims

1. A method for extracting vanadium and dephosphorizing vanadium from vanadium-containing molten iron, characterized in that: The steps include: S1, providing a first vanadium-containing molten iron, performing down-gun blowing on the first vanadium-containing molten iron, adding iron oxide in batches during the blowing process, and obtaining a first steel slag after the initial blowing; pouring out the first steel slag, crushing it after cooling, and sorting it to obtain a first vanadium-containing magnetic material and a first phosphorus-containing non-magnetic material; S2, providing a second vanadium-containing molten iron, performing down-gun blowing on the second vanadium-containing molten iron, adding the first vanadium-containing magnetic material and / or iron oxide in batches during the blowing process, and obtaining a second steel slag after the initial blowing; pouring out the second steel slag, crushing it after cooling, and sorting it to obtain a second vanadium-containing magnetic material and a second phosphorus-containing non-magnetic material; accordingly, the obtained second vanadium-containing magnetic material is used for blowing of a third vanadium-containing molten iron, until, SN, providing an Nth vanadium-containing molten iron, blowing the Nth vanadium-containing molten iron under a gun, adding an N-1th vanadium-containing magnetic material and / or iron oxide in batches during the blowing process, and obtaining an Nth steel slag after the initial blowing; pouring out the Nth steel slag, crushing it after cooling, and sorting it to obtain an Nth vanadium-containing magnetic material and an Nth phosphorus-containing non-magnetic material; Said N≥2; The basicity of the first steel slag, the second steel slag and the Nth steel slag is 1.3-1.5; The metallic iron content in the first steel slag, the second steel slag and the Nth steel slag is 4-12% by mass.

2. The method for extracting vanadium and dephosphorizing vanadium from vanadium-containing molten iron according to claim 1, characterized in that: If the vanadium content in the Nth vanadium-containing molten iron is 0.15-0.4 mass %, then N=2, and the vanadium pentoxide content in the Nth vanadium-containing magnetic material is ≥15 mass %.

3. The method for extracting vanadium and dephosphorizing vanadium from vanadium-containing molten iron according to claim 1, characterized in that: If the vanadium content in the Nth vanadium-containing iron water is 0.06-0.15 mass %, then 3≤N≤5, and the vanadium pentoxide content in the Nth vanadium-containing magnetic material is ≥8 mass %.

4. The method for extracting vanadium and dephosphorizing vanadium from vanadium-containing molten iron according to claim 1, characterized in that: The content of metallic iron in the first steel slag, the second steel slag and the Nth steel slag is 5-10% by mass.

5. The method for extracting vanadium and dephosphorizing vanadium from vanadium-containing molten iron according to claim 1, characterized in that: The content of MgO in the first steel slag, the second steel slag and the Nth steel slag is 0-5% by mass.

6. The method for extracting vanadium and dephosphorizing vanadium from vanadium-containing molten iron according to claim 1, characterized in that: The lower lance blowing adopts a low lance position and high oxygen supply intensity blowing process, wherein the low lance position is 100-200mm lower than the lance position in the early stage of blowing in the conventional process, and the high oxygen supply intensity is ≥3.0m / (min·t); the separation includes magnetic separation or gravity separation.