A moisture-heat-resistant high-transmittance polarizing film and a preparation method thereof

By using the combined technology of aminosilane coupling agent and acrylic pressure-sensitive adhesive in the PVA layer of the polarizer, the problem of insufficient moisture and heat resistance of existing polarizers in high-humidity and high-heat environments is solved, and high light transmittance and moisture-heat resistance are achieved. The effect is to extend the service life and reduce costs.

CN117518330BActive Publication Date: 2024-10-22HUNAN POLTECH OPTO-ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311468697.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-07
Publication Date
2024-10-22
Estimated Expiration
2043-11-07

AI Technical Summary

Technical Problem

Existing polarizers have insufficient resistance to moisture and heat in high-humidity and high-heat environments, making it difficult to meet application requirements in complex environments.

Method used

By using an aminosilane coupling agent in the PVA layer for modification, combined with the formula design of the acrylic pressure-sensitive adhesive, including ingredients such as vinyl acetate and maleimide, the bonding strength and heat resistance are improved, while the process is optimized. Prepare polarizer.

Benefits of technology

It significantly improves the heat and humidity resistance and light transmittance of the polarizer, prolongs its service life, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004534359070000091
    Figure BDA0004534359070000091
Patent Text Reader

Abstract

The present invention relates to the technical field of optical materials, and in particular to a moisture-heat-resistant high-transmittance polarizer and a preparation method thereof, the method comprising the following steps: step S1: modifying a PVA layer; step S2: preparing an acrylic pressure-sensitive adhesive; step S3: laminating a TAC layer; and step S4: preparing a polarizer. The present invention uses a silane coupling agent and a formula design of an acrylic pressure-sensitive adhesive to prepare a moisture-heat-resistant high-transmittance polarizer through a simple process, and synergistically improves the moisture-heat-resistant performance and light-transmittance performance of the polarizer. The method is simple and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of optical materials, and in particular to a moisture-heat-resistant high-transmittance polarizing sheet and a preparation method thereof. Background Art

[0002] Polarizer is a special optical film device that only allows light to pass in a certain direction. It is mainly composed of a polarizing layer (PVA), triacetate film (TAC), adhesive, release film and protective film. In today's electronic age, polarizers are not only widely used in LCD screens such as mobile phones, computers, and televisions, but also in display instruments such as vehicle-mounted industrial control systems, projectors, and outdoor testing instruments. The application is becoming more and more extensive, and the requirements for polarizers have also expanded from conventional conditions to complex environments such as high humidity and high heat. Therefore, as the main material of display instruments, polarizers also need to have the performance of high temperature and high humidity resistance.

[0003] However, current polarizers usually use a PVA glue layer to compound the PVA layer. Although the light transmittance is good, the heat resistance, especially the moisture and heat resistance, is insufficient, and the use of acrylic glue cannot guarantee the realization of high light transmittance. Therefore, the performance of the polarizer provided by the prior art needs to be improved. Summary of the invention

[0004] In view of the above problems, the present invention can simultaneously solve the problems of moisture and heat resistance and high light transmittance of the polarizer by adjusting the combination of formula and process, thereby extending the service life of the polarizer and reducing costs.

[0005] Specifically, the present invention provides a method for preparing a moisture-heat-resistant high-transmittance polarizing film, the method comprising the following steps:

[0006] Step S1: Modification of PVA layer

[0007] An aminosilane coupling agent ethanol solution is coated on both sides of the PVA layer, and the layer is dried for standby use to obtain a modified PVA layer;

[0008] Wherein, the amount of aminosilane coupling agent is 1.2-1.8% of the mass of the PVA layer;

[0009] Step S2: Preparation of acrylic pressure-sensitive adhesive

[0010] Prepare the following raw materials: 7-10 parts of methyl acrylate, 18-25 parts of isooctyl acrylate, 3-5 parts of acrylic acid, 27-37 parts of vinyl acetate, 0.15-0.3 parts of azo initiator, 6-10 parts of maleimide and 0.01-0.015 parts of mercaptan chain transfer agent;

[0011] Add the above raw materials and an appropriate amount of ethyl acetate into a reaction container for reaction, and cool to obtain an acrylic acid copolymer;

[0012] The acrylic copolymer, isocyanate and ethyl acetate obtained above are mixed to obtain an acrylic pressure-sensitive adhesive, wherein the acrylic copolymer is 45-61 parts, the isocyanate crosslinking agent is 0.15-0.3 parts, and the ethyl acetate is 60-77 parts;

[0013] Step S3: Laminating TAC layer

[0014] Apply the acrylic pressure-sensitive adhesive on one side of the modified PVA layer, adhere the TAC layer after drying and ripen, and then repeat the above process on the other side;

[0015] Step S4: Preparation of polarizer

[0016] Similarly, the acrylic pressure-sensitive adhesive is coated on the surface of the protective film and the release film, dried and aged, and then respectively attached to the two sides of the TAC layer, and cut to obtain a polarizer.

[0017] The aminosilane coupling agent includes one or two of gamma-aminoethyltriethoxysilane and gamma-aminopropyltriethoxysilane.

[0018] Preferably, the raw material composition of the synthetic acrylic copolymer is as follows:

[0019] 7.5-9.5 parts of methyl acrylate, 18.5-24.5 parts of isooctyl acrylate, 3.5-4.8 parts of acrylic acid, 27.5-36.5 parts of vinyl acetate, 0.15-0.3 parts of azo initiator, 7-9 parts of maleimide and 0.01-0.015 parts of thiol chain transfer agent.

[0020] Preferably, the composition of the acrylic pressure-sensitive adhesive is as follows:

[0021] 46.5-60.5 parts of acrylic copolymer, 0.15-0.3 parts of isocyanate crosslinking agent, and 60-76.5 parts of ethyl acetate.

[0022] Preferably, the acrylic acid copolymer is reacted under nitrogen protection.

[0023] Preferably, the acrylic acid copolymer is obtained by reacting at 60-75° C. for 6-10 h.

[0024] Preferably, the azo initiator includes one or both of azobisisobutyronitrile and azobisisoheptanenitrile.

[0025] Preferably, the mercaptan chain transfer agent includes one or both of dodecyl mercaptan and n-decyl mercaptan.

[0026] Preferably, the isocyanate cross-linking agent includes one or more of toluene diisocyanate, hexamethylene diisocyanate, and isophorone diisocyanate.

[0027] The present invention also provides a polarizer, which is prepared by the above method.

[0028] The present invention also provides an application of an acrylic pressure-sensitive adhesive, which is used for preparing the above-mentioned polarizer.

[0029] The present invention also provides an application of an acrylic pressure-sensitive adhesive, which can improve the moisture and heat resistance and light transmittance of a polarizer.

[0030] Compared with the prior art, the moisture-heat-resistant high-transmittance polarizing film of the present invention has the following beneficial effects:

[0031] (1) Silane coupling agents can improve the interfacial bonding ability of different materials. Aminosilane coupling agents are preferred in the present invention. The silanol group at one end can react with the OH group of the PVA layer, and the amino group at one end can cross-link with isocyanate, so that the acrylic glue and the PVA layer also undergo chemical bond cross-linking, greatly improving the bonding strength of the PVA layer. In addition, this cross-linking can effectively protect the PVA layer better, better resist the erosion of "moisture" on the PVA layer in a hot and humid environment, and obtain excellent hot and humid resistance.

[0032] (2) The layers of the polarizer are bonded with PVA glue or acrylic glue. Compared with PVA glue, acrylic glue has good solvent resistance, especially water resistance and temperature resistance. However, the inventors found that the corresponding light transmission performance will be affected and is not as good as PVA glue. After a large number of experiments, it was found that adding a certain amount of vinyl acetate can effectively improve the performance and achieve satisfactory polarization and light transmission performance. On this basis, adding an appropriate amount of maleimide can further improve the heat resistance of the polarizer.

[0033] (3) The present invention uses an aminosilane coupling agent in combination with a formula design of an acrylic pressure-sensitive adhesive to prepare a moisture-heat-resistant and highly transmittance polarizer through a simple process, thereby synergistically improving the moisture-heat resistance and light transmittance of the polarizer. The method is simple and has broad application prospects. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] A method for preparing a moisture-heat-resistant high-transmittance polarizing film, the method steps are as follows:

[0037] Step S1: Modification of PVA layer

[0038] A γ-aminopropyl triethoxysilane ethanol solution is coated on both sides of the PVA layer, and the layer is dried for later use to obtain a modified PVA layer;

[0039] Wherein, the amount of γ-aminopropyltriethoxysilane is 1.5% of the mass of the PVA layer;

[0040] Step S2: Preparation of acrylic pressure-sensitive adhesive

[0041] Prepare the following raw materials: 8 parts of methyl acrylate, 20 parts of isooctyl acrylate, 4 parts of acrylic acid, 30 parts of vinyl acetate, 0.2 parts of azobisisobutyronitrile, 7.5 parts of maleimide and 0.01 parts of dodecyl mercaptan;

[0042] The above raw materials and an appropriate amount of ethyl acetate were added into a reaction vessel, reacted at 65-70° C. for 8 h under nitrogen protection, and cooled to obtain an acrylic acid copolymer;

[0043] The acrylic copolymer, toluene diisocyanate and ethyl acetate obtained above are mixed to obtain an acrylic pressure-sensitive adhesive, wherein the acrylic copolymer is 50 parts, the toluene diisocyanate is 0.2 parts and the ethyl acetate is 65 parts;

[0044] Step S3: Laminating TAC layer

[0045] Apply the acrylic pressure-sensitive adhesive on one side of the modified PVA layer, adhere the TAC layer after drying and ripen, and then repeat the above process on the other side;

[0046] Step S4: Preparation of polarizer

[0047] Similarly, the acrylic pressure-sensitive adhesive is coated on the surface of the protective film and the release film, dried and aged, and then respectively attached to the two sides of the TAC layer, and cut to obtain a polarizer.

[0048] Example 2

[0049] A method for preparing a moisture-heat-resistant high-transmittance polarizing film, the method steps are as follows:

[0050] Step S1: Modification of PVA layer

[0051] A γ-aminopropyl triethoxysilane ethanol solution is coated on both sides of the PVA layer, and the layer is dried for later use to obtain a modified PVA layer;

[0052] Wherein, the amount of γ-aminopropyltriethoxysilane is 1.5% of the mass of the PVA layer;

[0053] Step S2: Preparation of acrylic pressure-sensitive adhesive

[0054] Prepare the following raw materials: 9.5 parts of methyl acrylate, 24.5 parts of isooctyl acrylate, 5 parts of acrylic acid, 36.5 parts of vinyl acetate, 0.25 parts of azobisisobutyronitrile, 9 parts of maleimide and 0.015 parts of dodecyl mercaptan;

[0055] The above raw materials and an appropriate amount of ethyl acetate were added into a reaction vessel, reacted at 65-70° C. for 8 h under nitrogen protection, and cooled to obtain an acrylic acid copolymer;

[0056] The acrylic copolymer, toluene diisocyanate and ethyl acetate obtained above were mixed to obtain an acrylic pressure-sensitive adhesive, wherein the acrylic copolymer was 60.5 parts, the toluene diisocyanate was 0.3 parts and the ethyl acetate was 76.5 parts;

[0057] Step S3: Laminating TAC layer

[0058] Apply the acrylic pressure-sensitive adhesive on one side of the modified PVA layer, adhere the TAC layer after drying and ripen, and then repeat the above process on the other side;

[0059] Step S4: Preparation of polarizer

[0060] Similarly, the acrylic pressure-sensitive adhesive is coated on the surface of the protective film and the release film, dried and aged, and then respectively attached to the two sides of the TAC layer, and cut to obtain a polarizer.

[0061] Example 3

[0062] A method for preparing a moisture-heat-resistant high-transmittance polarizing film, the method steps are as follows:

[0063] Step S1: Modification of PVA layer

[0064] A γ-aminopropyl triethoxysilane ethanol solution is coated on both sides of the PVA layer, and the layer is dried for later use to obtain a modified PVA layer;

[0065] Wherein, the amount of γ-aminopropyltriethoxysilane is 1.5% of the mass of the PVA layer;

[0066] Step S2: Preparation of acrylic pressure-sensitive adhesive

[0067] Prepare the following raw materials: 7.5 parts of methyl acrylate, 18.5 parts of isooctyl acrylate, 3.5 parts of acrylic acid, 27.5 parts of vinyl acetate, 0.18 parts of azobisisobutyronitrile, 7 parts of maleimide and 0.01 parts of dodecyl mercaptan;

[0068] The above raw materials and an appropriate amount of ethyl acetate were added into a reaction vessel, reacted at 65-70° C. for 8 h under nitrogen protection, and cooled to obtain an acrylic acid copolymer;

[0069] The acrylic copolymer, toluene diisocyanate and ethyl acetate obtained above are mixed to obtain an acrylic pressure-sensitive adhesive, wherein the acrylic copolymer is 46.5 parts, toluene diisocyanate is 0.15 parts and ethyl acetate is 60 parts;

[0070] Step S3: Laminating TAC layer

[0071] Apply the acrylic pressure-sensitive adhesive on one side of the modified PVA layer, adhere the TAC layer after drying and ripen, and then repeat the above process on the other side;

[0072] Step S4: Preparation of polarizer

[0073] Similarly, the acrylic pressure-sensitive adhesive is coated on the surface of the protective film and the release film, dried and aged, and then respectively attached to the two sides of the TAC layer, and cut to obtain a polarizer.

[0074] Comparative Example 1

[0075] A method for preparing a moisture-heat-resistant high-transmittance polarizing film, the method steps are as follows:

[0076] Step S1: Preparation of PVA layer

[0077] Prepare an unmodified PVA layer for later use;

[0078] Step S2: Preparation of acrylic pressure-sensitive adhesive

[0079] Prepare the following raw materials: 8 parts of methyl acrylate, 20 parts of isooctyl acrylate, 4 parts of acrylic acid, 30 parts of vinyl acetate, 0.2 parts of azobisisobutyronitrile, 7.5 parts of maleimide and 0.01 parts of dodecyl mercaptan;

[0080] The above raw materials and an appropriate amount of ethyl acetate were added into a reaction vessel, reacted at 65-70° C. for 8 h under nitrogen protection, and cooled to obtain an acrylic acid copolymer;

[0081] The acrylic copolymer, toluene diisocyanate and ethyl acetate obtained above are mixed to obtain an acrylic pressure-sensitive adhesive, wherein the acrylic copolymer is 50 parts, the toluene diisocyanate is 0.2 parts and the ethyl acetate is 65 parts;

[0082] Step S3: Laminating TAC layer

[0083] Apply the acrylic pressure-sensitive adhesive on one side of the modified PVA layer, adhere the TAC layer after drying and ripen, and then repeat the above process on the other side;

[0084] Step S4: Preparation of polarizer

[0085] Similarly, the acrylic pressure-sensitive adhesive is coated on the surface of the protective film and the release film, dried and aged, and then respectively attached to the two sides of the TAC layer, and cut to obtain a polarizer.

[0086] Comparative Example 2

[0087] A method for preparing a moisture-heat-resistant high-transmittance polarizing film, the method steps are as follows:

[0088] Step S1: Modification of PVA layer

[0089] Vinyl trimethoxysilane ethanol solution is coated on both sides of the PVA layer, and dried for standby use to obtain a modified PVA layer;

[0090] Wherein, the amount of vinyl trimethoxy silane is 1.5% of the mass of the PVA layer;

[0091] Step S2: Preparation of acrylic pressure-sensitive adhesive

[0092] Prepare the following raw materials: 8 parts of methyl acrylate, 20 parts of isooctyl acrylate, 4 parts of acrylic acid, 30 parts of vinyl acetate, 0.2 parts of azobisisobutyronitrile, 7.5 parts of maleimide and 0.01 parts of dodecyl mercaptan;

[0093] The above raw materials and an appropriate amount of ethyl acetate were added into a reaction vessel, reacted at 65-70° C. for 8 h under nitrogen protection, and cooled to obtain an acrylic acid copolymer;

[0094] The acrylic copolymer, toluene diisocyanate and ethyl acetate obtained above are mixed to obtain an acrylic pressure-sensitive adhesive, wherein the acrylic copolymer is 50 parts, the toluene diisocyanate is 0.2 parts and the ethyl acetate is 65 parts;

[0095] Step S3: Laminating TAC layer

[0096] Apply the acrylic pressure-sensitive adhesive on one side of the modified PVA layer, adhere the TAC layer after drying and ripen, and then repeat the above process on the other side;

[0097] Step S4: Preparation of polarizer

[0098] Similarly, the acrylic pressure-sensitive adhesive is coated on the surface of the protective film and the release film, dried and aged, and then respectively attached to the two sides of the TAC layer, and cut to obtain a polarizer.

[0099] Comparative Example 3

[0100] A method for preparing a moisture-heat-resistant high-transmittance polarizing film, the method steps are as follows:

[0101] Step S1: Modification of PVA layer

[0102] A γ-aminopropyl triethoxysilane ethanol solution is coated on both sides of the PVA layer, and the layer is dried for later use to obtain a modified PVA layer;

[0103] Wherein, the amount of γ-aminopropyltriethoxysilane is 1.5% of the mass of the PVA layer;

[0104] Step S2: Preparation of acrylic pressure-sensitive adhesive

[0105] Prepare the following raw materials: 8 parts of methyl acrylate, 20 parts of isooctyl acrylate, 30 parts of acrylic acid, 4 parts of vinyl acetate, 0.2 parts of azobisisobutyronitrile, 7.5 parts of maleimide and 0.01 parts of dodecyl mercaptan;

[0106] The above raw materials and an appropriate amount of ethyl acetate were added into a reaction vessel, reacted at 65-70° C. for 8 h under nitrogen protection, and cooled to obtain an acrylic acid copolymer;

[0107] The acrylic copolymer, toluene diisocyanate and ethyl acetate obtained above are mixed to obtain an acrylic pressure-sensitive adhesive, wherein the acrylic copolymer is 50 parts, the toluene diisocyanate is 0.2 parts and the ethyl acetate is 65 parts;

[0108] Step S3: Laminating TAC layer

[0109] Apply the acrylic pressure-sensitive adhesive on one side of the modified PVA layer, adhere the TAC layer after drying and ripen, and then repeat the above process on the other side;

[0110] Step S4: Preparation of polarizer

[0111] Similarly, the acrylic pressure-sensitive adhesive is coated on the surface of the protective film and the release film, dried and aged, and then respectively attached to the two sides of the TAC layer, and cut to obtain a polarizer.

[0112] Comparative Example 4

[0113] A method for preparing a moisture-heat-resistant high-transmittance polarizing film, the method steps are as follows:

[0114] Step S1: Modification of PVA layer

[0115] A γ-aminopropyl triethoxysilane ethanol solution is coated on both sides of the PVA layer, and the layer is dried for later use to obtain a modified PVA layer;

[0116] Wherein, the amount of γ-aminopropyltriethoxysilane is 1.5% of the mass of the PVA layer;

[0117] Step S2: Preparation of acrylic pressure-sensitive adhesive

[0118] Prepare the following raw materials: 8 parts of methyl acrylate, 20 parts of isooctyl acrylate, 4 parts of acrylic acid, 30 parts of vinyl acetate, 0.2 parts of azobisisobutyronitrile and 0.01 parts of dodecyl mercaptan;

[0119] The above raw materials and an appropriate amount of ethyl acetate were added into a reaction vessel, reacted at 65-70° C. for 8 h under nitrogen protection, and cooled to obtain an acrylic acid copolymer;

[0120] The acrylic copolymer, toluene diisocyanate and ethyl acetate obtained above are mixed to obtain an acrylic pressure-sensitive adhesive, wherein the acrylic copolymer is 50 parts, the toluene diisocyanate is 0.2 parts and the ethyl acetate is 65 parts;

[0121] Step S3: Laminating TAC layer

[0122] Apply the acrylic pressure-sensitive adhesive on one side of the modified PVA layer, adhere the TAC layer after drying and ripen, and then repeat the above process on the other side;

[0123] Step S4: Preparation of polarizer

[0124] Similarly, the acrylic pressure-sensitive adhesive is coated on the surface of the protective film and the release film, dried and aged, and then respectively attached to the two sides of the TAC layer, and cut to obtain a polarizer.

[0125] Comparative Example 5

[0126] A method for preparing a moisture-heat-resistant high-transmittance polarizing film, the method steps are as follows:

[0127] Step S1: Modification of PVA layer

[0128] A γ-aminopropyl triethoxysilane ethanol solution is coated on both sides of the PVA layer, and the layer is dried for later use to obtain a modified PVA layer;

[0129] Wherein, the amount of γ-aminopropyltriethoxysilane is 1.5% of the mass of the PVA layer;

[0130] Step S2: Laminating TAC layer

[0131] Apply PVA glue to one side of the modified PVA layer, attach the TAC layer, dry it, and then repeat the above process on the other side;

[0132] Step S3: Preparation of polarizer

[0133] Similarly, commercially available acrylic pressure-sensitive adhesive is coated on the surface of the protective film and the release film, dried and cured, and then respectively attached to the two sides of the above-mentioned TAC layer, and cut to obtain a polarizer.

[0134] Performance Testing

[0135] The polarization degree and transmittance of the obtained polarizer were tested, and then the moisture and heat resistance of the polarizer was tested. After placing it in a 70°C×95%RH environment for 500 hours, the polarization degree and transmittance were also tested, and the polarizer was visually inspected for deformation, mainly for warping. The test results are shown in Table 1.

[0136] Table 1: Polarizer performance test

[0137]

[0138] It can be seen from the above that the polarizers obtained in Examples 1-3 have good moisture and heat resistance, while no silane coupling agent is used in Comparative Example 1, and different silane coupling agents are used in Comparative Example 2, and the corresponding polarizers have poor moisture and heat resistance, and there is warping in Comparative Example 1. Vinyl acetate and maleimide components have obvious improvements on the adhesion and heat resistance of the PVA layer. The vinyl acetate content in Comparative Example 3 is low, and no maleimide is added in Comparative Example 4, and the moisture and heat resistance of the obtained polarizer is not satisfactory.

[0139] In Comparative Example 5, common commercially available PVA glue is used. Although the light transmittance is good, the moisture and heat resistance is poor. PVA easily absorbs water, thus affecting the performance of the polarizer.

[0140] Those skilled in the art will appreciate that the embodiments described above are only a portion of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative work are within the scope of protection of the present invention.

Claims

1. A method for preparing a moisture-heat-resistant high-transmittance polarizing film, the method comprising the following steps: Step S1: Modification of PVA layer An aminosilane coupling agent ethanol solution is coated on both sides of the PVA layer, and the layer is dried for standby use to obtain a modified PVA layer; in, The dosage of aminosilane coupling agent is 1.2-1.8% of the mass of PVA layer; Step S2: Preparation of acrylic pressure-sensitive adhesive Prepare the following raw materials: 7-10 parts of methyl acrylate, 18-25 parts of isooctyl acrylate, 3-5 parts of acrylic acid, 27-37 parts of vinyl acetate, 0.15-0.3 parts of azo initiator, 6-10 parts of maleimide and 0.01-0.015 parts of mercaptan chain transfer agent; Add the above raw materials and an appropriate amount of ethyl acetate into a reaction container for reaction, and cool to obtain an acrylic acid copolymer; The obtained acrylic copolymer, isocyanate and ethyl acetate are mixed to obtain an acrylic pressure-sensitive adhesive, wherein the acrylic copolymer comprises 45-61 parts, the isocyanate crosslinking agent comprises 0.15-0.3 parts and the ethyl acetate comprises 60-77 parts; Step S3: Laminating TAC layer Apply the acrylic pressure-sensitive adhesive on one side of the modified PVA layer, adhere the TAC layer after drying and ripen, and then repeat the above process on the other side; Step S4: Preparation of polarizer The acrylic pressure-sensitive adhesive is coated on the surfaces of the protective film and the release film, dried and aged, and then respectively attached to the two sides of the TAC layer, and cut to obtain a polarizer.

2. The preparation method according to claim 1, wherein the aminosilane coupling agent comprises one or both of γ-aminoethyltriethoxysilane and γ-aminopropyltriethoxysilane.

3. The preparation method according to claim 1, wherein the raw materials for synthesizing the acrylic acid copolymer are as follows: 7.5-9.5 parts of methyl acrylate, 18.5-24.5 parts of isooctyl acrylate, 3.5-4.8 parts of acrylic acid, 27.5-36.5 parts of vinyl acetate, 0.15-0.3 parts of azo initiator, 7-9 parts of maleimide and 0.01-0.015 parts of thiol chain transfer agent.

4. The preparation method according to claim 1, wherein the acrylic pressure-sensitive adhesive comprises the following components: 46.5-60.5 parts of acrylic copolymer, 0.15-0.3 parts of isocyanate crosslinking agent, and 60-76.5 parts of ethyl acetate.

5. The preparation method according to claim 1, wherein the acrylic acid copolymer is reacted under nitrogen protection.

6. The preparation method according to claim 1, wherein the acrylic acid copolymer is obtained by reacting at 60-75°C for 6-10 hours.

7. The preparation method according to claim 1, wherein the azo initiator comprises one or both of azobisisobutyronitrile and azobisisoheptanenitrile.

8. The preparation method according to claim 1, wherein the mercaptan chain transfer agent comprises one or both of dodecyl mercaptan and n-decyl mercaptan.

9. The preparation method according to claim 1, wherein the isocyanate cross-linking agent comprises one or more of toluene diisocyanate, hexamethylene diisocyanate, and isophorone diisocyanate.

10. A polarizer, characterized in that the polarizer is prepared by the method described in any one of claims 1 to 9.