Fluorosilicone modified acrylate resin, smear-resistant coating and preparation method thereof
Through the combination of fluorosilicone-modified acrylate resin, the problem that it is difficult for the coating to be stain-resistant, wear-resistant, high-temperature resistant and flexible at the same time is solved, thereby improving the overall performance of the coating and extending its service life.
Patent Information
- Application Number
- CN202311551491.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-21
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-11-21
AI Technical Summary
It is difficult to improve the coating's stain resistance, wear resistance, high temperature resistance and flexibility at the same time with the existing technology, and there is a lack of comprehensive performance coating solutions.
Using fluorosilicone modified acrylate resin, through the combination of styrene, aliphatic polyurethane acrylate, hydroxyl- and carboxyl-containing acrylate monomers and fluorosilicone functional monomers, a smear-resistant, high-temperature-resistant, It can be used to prepare coatings with good grinding and toughness, combined with other additives.
It achieves the coating's comprehensive properties of long-lasting stain resistance, high temperature resistance, wear resistance and good flexibility, extending the service life of the coating.
Smart Images

Figure SMS_5 
Figure QLYQS_1 
Figure QLYQS_2
Abstract
Description
Technical Field
[0001] The invention relates to the field of coatings, and in particular to a fluorosilicone modified acrylate resin, a smear-resistant coating and a preparation method thereof. Background Art
[0002] In recent years, many consumers' coating requirements for electronic consumer products are no longer limited to the appearance effect, and the performance requirements for the product surface coating are also increasing. Among them, the coating's long-lasting resistance to smearing, wear resistance, high temperature resistance, and good flexibility are currently the more popular coating surface properties.
[0003] At present, the relevant technologies can achieve a single anti-smear effect, a wear-resistant effect, a high-temperature resistance effect, or a flexibility effect. However, a solution for simultaneously improving the coating's long-lasting anti-smear, abrasion resistance, high-temperature resistance, and flexibility has not yet been studied. Summary of the invention
[0004] In order to improve the problem that related technologies are difficult to simultaneously improve the coating's durability in terms of smear resistance, wear resistance, high temperature resistance, and flexibility, the present application provides a fluorosilicone-modified acrylate resin, a smear-resistant coating, and a preparation method thereof.
[0005] In the first aspect, the present application provides a fluorosilicone modified acrylate resin adopts the following technical solution:
[0006] A fluorine-silicon modified acrylate resin comprises the following raw materials in parts by weight:
[0007] Styrene: 100-150 parts
[0008] Aliphatic polyurethane acrylate: 200-300 parts
[0009] Hydroxyl-containing acrylate monomer: 150-250 parts
[0010] Carboxyl-containing acrylic monomer: 20-50 parts
[0011] Fluorosilicone functional monomer: 50-150 parts
[0012] Initiator: 5-8 parts
[0013] Chain transfer agent: 1-3 parts
[0014] Alcohol solvent: 28-35 parts
[0015] Water: 5-12 parts.
[0016] Fluorosilicon-modified acrylate resin is prepared by combining styrene, aliphatic polyurethane acrylate, hydroxyl-containing acrylate monomer, carboxyl-containing acrylic monomer and fluorosilicone functional monomer. The fluorosilicone-modified acrylate resin has the characteristics of good durability and resistance to smearing. At the same time, it also has the advantages of high temperature resistance, wear resistance and good toughness. The fluorosilicone-modified acrylate resin is combined with other basic additives to prepare coatings, and a coating with long-lasting resistance to smearing, wear resistance, high temperature resistance and good flexibility can be obtained.
[0017] Optionally, the fluorine-silicon functional monomer includes a fluorine-containing functional monomer and a silicon-containing functional monomer, and the weight ratio of the fluorine-containing functional monomer to the silicon-containing functional monomer is (1-2):3;
[0018] The fluorine-containing functional monomer is selected from any one of hexafluorobutyl methacrylate and dodecafluoroheptyl methacrylate or a combination of two thereof; the silicon-containing functional monomer is selected from any one of vinyltrimethoxysilane and vinyltriethoxysilane or a combination of two thereof.
[0019] The fluorine-containing functional monomer and the silicon-containing functional monomer react with other acrylate monomers to bond in the acrylic resin chain segment, which can effectively improve the long-lasting smear resistance of the fluorine-silicon modified acrylate resin. In addition, when the weight ratio of the fluorine-containing functional monomer to the silicon-containing functional monomer is (1-2):3, it is beneficial to further improve the high temperature resistance and wear resistance of the fluorine-silicon modified acrylate resin.
[0020] Optionally, the fluorosilicone functional monomer is selected from any one of hexacarbon perfluoropolyether trimethoxysilane and hexacarbon perfluoropolyether triethoxysilane, or a combination of the two; wherein the structural formula of the hexacarbon perfluoropolyether trimethoxysilane is as follows:
[0021] .
[0022] The structural formula of the hexacarbon perfluoropolyether triethoxysilane is as follows:
[0023] .
[0024] When the fluorosilicone functional monomer is any one of hexafluoropolyether trimethoxysilane and hexafluoropolyether triethoxysilane or a combination of the two, not only can a fluorosilicone modified acrylate resin with durable smear resistance be obtained, but the high temperature resistance and toughness of the fluorosilicone modified acrylate resin can also be further improved.
[0025] Optionally, the aliphatic polyurethane acrylate is selected from any one of tetrafunctional aliphatic polyurethane acrylate, pentafunctional aliphatic polyurethane acrylate, hexafunctional aliphatic polyurethane acrylate, or a combination of several thereof.
[0026] Aliphatic polyurethane acrylates Using aliphatic polyurethane acrylates with 4-6 functionalities is beneficial to further improve the high temperature resistance and wear resistance of the fluorosilicone modified acrylate resin.
[0027] Optionally, the hydroxyl-containing acrylate monomer is selected from any one of hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxyethyl acrylate, and hydroxypropyl acrylate, or a combination of several of them.
[0028] Optionally, the carboxyl-containing acrylic acid monomer is selected from any one of acrylic acid and methacrylic acid or a combination of the two.
[0029] Optionally, the initiator is selected from any one of azobisisobutyronitrile and azobisisoheptanenitrile.
[0030] Optionally, the chain transfer agent is a hydroxyl chain transfer agent.
[0031] Preferably, the hydroxyl chain transfer agent is any one of mercaptoethanol, mercaptopropanol, and 2-hydroxyethyl mercaptopropionate.
[0032] Optionally, the alcohol solvent is selected from any one of isopropanol and hexafluoroisopropanol or a combination of the two, preferably a combination of isopropanol and hexafluoroisopropanol, and the weight ratio of isopropanol to hexafluoroisopropanol is (1-2):3.
[0033] In the second aspect, the present application provides a method for preparing a fluorosilicone modified acrylate resin using the following technical solution:
[0034] A method for preparing a fluorine-silicon modified acrylate resin comprises the following steps:
[0035] uniformly mixing an alcohol solvent with water to prepare a mixed solution;
[0036] Add 30-50% of the total weight of the mixed solution to styrene, stir, and then continue to add aliphatic polyurethane acrylate, stir evenly, to obtain a first monomer solution;
[0037] Adding hydroxyl-containing acrylate monomer, carboxyl-containing acrylic acid monomer and fluorosilicone functional monomer to the remaining mixed solution, heating to 40-50° C., reacting for 1-1.5 hours, to obtain a second monomer solution;
[0038] The first monomer solution, the second monomer solution and the chain transfer agent are uniformly mixed, and then the initiator is added dropwise. The reaction temperature is controlled at 65-75° C. and the reaction is carried out for 2-4 hours to obtain a fluorosilicone modified acrylate resin.
[0039] When the fluorosilicone modified acrylate resin is prepared by the above method, it is beneficial to further improve the durable stain resistance of the fluorosilicone modified acrylate resin.
[0040] In a third aspect, the present application provides a smear-resistant coating that adopts the following technical solution:
[0041] A smear-resistant coating comprising the following raw materials in percentage by weight:
[0042] Fluorosilicone modified acrylate resin: 35-45%
[0043] Trimethylolpropane triacrylate: 4-6%
[0044] Photoinitiator: 1-3%
[0045] Leveling agent: 0.1-0.2%
[0046] Solvent: Balance.
[0047] The fluorosilicone modified acrylate resin is selected from any one of the fluorosilicone modified acrylate resins described above.
[0048] Fluorosilicone-modified acrylate resin is used together with trimethylolpropane triacrylate, a photoinitiator, a leveling aid, etc. to prepare a smear-resistant coating. The coating has the characteristics of strong wettability and good leveling property. After the coating is cured under the catalytic effect of light, the cured coating has the characteristics of good durability in smear resistance, high temperature resistance, wear resistance, and good toughness.
[0049] Optionally, the photoinitiator is photoinitiator TPO.
[0050] Optionally, the leveling aid is a silicone leveling agent, such as any one of polydimethylsiloxane, polymethylalkylsiloxane, and organic modified polysiloxane.
[0051] Adding silicone leveling agent can improve the leveling performance of the coating, reduce the occurrence of orange peel problems, and have good anti-cratering effect.
[0052] Optionally, the solvent is selected from hydrocarbons or esters.
[0053] In a fourth aspect, the present application provides a method for preparing a smear-resistant coating using the following technical solution:
[0054] A method for preparing a smear-resistant coating comprises the following steps:
[0055] Uniformly dispersing fluorosilicone-modified acrylate resin, trimethylolpropane triacrylate and a photoinitiator in a solvent to obtain a dispersed solution;
[0056] Add a leveling agent to the dispersed solution and stir evenly to obtain a smear-resistant coating.
[0057] The above method is used to prepare the smear-resistant coating, which is conducive to obtaining the smear-resistant coating with uniform dispersion and good leveling properties.
[0058] In summary, the technical solution of the present application includes at least the following beneficial effects:
[0059] (1) A fluorosilicone-modified acrylate resin is prepared by combining styrene, aliphatic polyurethane acrylate, a hydroxyl-containing acrylate monomer, a carboxyl-containing acrylic monomer and a fluorosilicone functional monomer. The fluorosilicone-modified acrylate resin has the characteristics of good durability and resistance to smearing. At the same time, it also has the advantages of high temperature resistance, wear resistance and good toughness.
[0060] (2) When the fluorosilicone functional monomer is any one of hexafluoropolyether trimethoxysilane and hexafluoropolyether triethoxysilane or a combination of the two, not only can a fluorosilicone modified acrylate resin with long-lasting anti-smearing performance be obtained, but the high temperature resistance and toughness of the fluorosilicone modified acrylate resin can also be further improved. DETAILED DESCRIPTION
[0061] The present application is further described in detail below in conjunction with specific experiments.
[0062] Example
[0063] [Example 1]
[0064] A fluorosilicone modified acrylate resin, comprising the following raw materials:
[0065] Styrene: 100kg;
[0066] Aliphatic polyurethane acrylate: 300kg; specifically, hexafunctional aliphatic polyurethane acrylate with a viscosity of 15000cps;
[0067] Hydroxyl-containing acrylate monomer: 150kg; specifically, hydroxyethyl acrylate;
[0068] Carboxyl-containing acrylic acid monomer: 50 kg; specifically, methacrylic acid;
[0069] Fluorosilicone functional monomer: 50kg; calculated on the basis of fluorosilicone functional monomer, the fluorosilicone functional monomer includes hexafluorobutyl methacrylate and vinyltrimethoxysilane, and the weight ratio of hexafluorobutyl methacrylate to vinyltrimethoxysilane is 1:3;
[0070] Initiator: 5kg; azobisisobutyronitrile is used;
[0071] Chain transfer agent: 1kg; mercaptoethanol is used;
[0072] Alcohol solvent: 28 kg; calculated as alcohol solvent, the alcohol solvent includes isopropanol and hexafluoroisopropanol, and the weight ratio of isopropanol to hexafluoroisopropanol is 2:3;
[0073] Water: 5kg.
[0074] In this embodiment, the preparation method of fluorine-silicon modified acrylate resin comprises the following steps:
[0075] S1, uniformly mixing an alcohol solvent and water to obtain a mixed solution;
[0076] S2, adding 40% of the total weight of the mixed solution to styrene, stirring, and then continuing to add aliphatic polyurethane acrylate, stirring evenly, to obtain a first monomer solution;
[0077] S3, adding a hydroxyl-containing acrylate monomer, a carboxyl-containing acrylic acid monomer, and a fluorosilicone functional monomer to the remaining mixed solution, heating to 45° C., and reacting for 1 hour to obtain a second monomer solution;
[0078] S4, uniformly mix the first monomer solution, the second monomer solution and the chain transfer agent, then dropwise add the initiator, control the reaction temperature at 70° C., react for 3 hours, and obtain a fluorosilicone-modified acrylate resin.
[0079] [Example 2]
[0080] A fluorosilicone modified acrylate resin, comprising the following raw materials:
[0081] Styrene: 125kg;
[0082] Aliphatic polyurethane acrylate: 250kg; specifically, hexafunctional aliphatic polyurethane acrylate with a viscosity of 15000cps;
[0083] Hydroxyl-containing acrylate monomer: 200 kg; specifically, hydroxyethyl acrylate is selected;
[0084] Carboxyl-containing acrylic acid monomer: 35 kg; specifically, methacrylic acid;
[0085] Fluorosilicone functional monomer: 100kg; calculated as fluorosilicone functional monomer, the fluorosilicone functional monomer includes hexafluorobutyl methacrylate and vinyltrimethoxysilane, and the weight ratio of hexafluorobutyl methacrylate to vinyltrimethoxysilane is 1:3;
[0086] Initiator: 6.5 kg; azobisisobutyronitrile is used;
[0087] Chain transfer agent: 2kg; mercaptoethanol is used;
[0088] Alcohol solvent: 32kg; calculated as alcohol solvent, the alcohol solvent includes isopropanol and hexafluoroisopropanol, and the weight ratio of isopropanol to hexafluoroisopropanol is 2:3;
[0089] Water: 8kg.
[0090] In this embodiment, the preparation method of fluorosilicone modified acrylate resin is the same as that in [Example 1].
[0091] [Example 3]
[0092] A fluorosilicone modified acrylate resin, comprising the following raw materials:
[0093] Styrene: 150kg;
[0094] Aliphatic polyurethane acrylate: 200kg; specifically, hexafunctional aliphatic polyurethane acrylate with a viscosity of 15000cps;
[0095] Hydroxyl-containing acrylate monomer: 250kg; specifically, hydroxyethyl acrylate;
[0096] Carboxyl-containing acrylic acid monomer: 20 kg; specifically, methacrylic acid;
[0097] Fluorosilicone functional monomer: 150kg; calculated as fluorosilicone functional monomer, the fluorosilicone functional monomer includes hexafluorobutyl methacrylate and vinyltrimethoxysilane, and the weight ratio of hexafluorobutyl methacrylate to vinyltrimethoxysilane is 1:3;
[0098] Initiator: 8kg; azobisisobutyronitrile is used;
[0099] Chain transfer agent: 3kg; mercaptoethanol is used;
[0100] Alcohol solvent: 35kg; calculated as alcohol solvent, the alcohol solvent includes isopropanol and hexafluoroisopropanol, and the weight ratio of isopropanol to hexafluoroisopropanol is 2:3;
[0101] Water: 12kg.
[0102] In this embodiment, the preparation method of fluorosilicone modified acrylate resin is the same as that in [Example 1].
[0103] [Example 4]
[0104] A fluorosilicone modified acrylate resin, which differs from [Example 2] in that the fluorosilicone functional monomer is different.
[0105] In this embodiment, the fluorine-silicon functional monomer is selected from hexacarbon perfluoropolyether trimethoxysilane, and the structural formula of hexacarbon perfluoropolyether trimethoxysilane is as follows:
[0106] .
[0107] [Example 5]
[0108] A fluorosilicone modified acrylate resin, which is different from [Example 2] in that the fluorosilicone functional monomer is hexafluoropolyether triethoxysilane, and the structural formula of hexafluoropolyether triethoxysilane is as follows:
[0109] .
[0110] [Example 6]
[0111] A fluorosilicone modified acrylate resin, which is different from [Example 5] in that the preparation method of the fluorosilicone modified acrylate resin is different.
[0112] In this embodiment, the preparation method of fluorine-silicon modified acrylate resin comprises the following steps:
[0113] uniformly mixing an alcohol solvent with water to prepare a mixed solution;
[0114] Add 40% of the total weight of the mixed solution to styrene, stir, then continue to add aliphatic polyurethane acrylate, hydroxyl-containing acrylate monomer and carboxyl-containing acrylic monomer, stir evenly, to obtain a first monomer solution;
[0115] Add the fluorine-silicon functional monomer to the remaining mixed solution, raise the temperature to 45° C., and react for 1 hour to obtain a second monomer solution;
[0116] The first monomer solution, the second monomer solution and the chain transfer agent were uniformly mixed, and then the initiator was added dropwise. The reaction temperature was controlled at 70° C. and the reaction was carried out for 3 hours to obtain a fluorosilicone-modified acrylate resin.
[0117] Comparative Example
[0118] [Comparative Example 1]
[0119] A fluorosilicone modified acrylate resin, which differs from [Example 5] in that:
[0120] The aliphatic polyurethane acrylate in step S2 is replaced by an equal amount of hydroxyethyl acrylate.
[0121] [Comparative Example 2]
[0122] A fluorosilicone modified acrylate resin, which differs from [Example 5] in that:
[0123] The styrene in step S2 is replaced by an equal amount of hexafunctional aliphatic polyurethane acrylate.
[0124] [Comparative Example 3]
[0125] A fluorosilicone modified acrylate resin, which differs from [Example 5] in that:
[0126] The carboxyl-containing acrylic acid monomer in step S3 is replaced by an equal amount of hydroxyethyl acrylate.
[0127] Application Examples
[0128]
Application Example 1
[0129] A smear-resistant coating comprising the following raw materials in percentage by weight:
[0130] Fluorosilicone modified acrylate resin: 35%, specifically the fluorine-silicone modified acrylate resin prepared in [Example 1];
[0131] Trimethylolpropane triacrylate: 4%;
[0132] Photoinitiator: 1%, specifically photoinitiator TPO;
[0133] Leveling agent: 0.1%, specifically polydimethylsiloxane;
[0134] Solvent: 59.9%, specifically ethyl acetate.
[0135] In this application example, the method for preparing the smear-resistant coating comprises the following steps:
[0136] Add fluorosilicone modified acrylate resin, trimethylolpropane triacrylate and photoinitiator into the solvent, stir at 500 r / min for 1 hour to obtain a dispersed solution;
[0137] Add a leveling agent to the dispersed solution and stir at 500 r / min for 20 min to obtain a smear-resistant coating.
[0138]
Application Example 2
[0139] A smear-resistant coating comprising the following raw materials in percentage by weight:
[0140] Fluorosilicone modified acrylate resin: 40%, specifically the fluorine-silicone modified acrylate resin prepared in [Example 1];
[0141] Trimethylolpropane triacrylate: 5%;
[0142] Photoinitiator: 2%, specifically photoinitiator TPO;
[0143] Leveling agent: 0.15%, specifically polydimethylsiloxane;
[0144] Solvent: 52.85%, specifically ethyl acetate.
[0145] In this application example, the preparation method of the smear-resistant coating is the same as that in [Application Example 1].
[0146]
Application Example 3
[0147] A smear-resistant coating comprising the following raw materials in percentage by weight:
[0148] Fluorosilicone modified acrylate resin: 45%, specifically the fluorine-silicone modified acrylate resin prepared in [Example 1];
[0149] Trimethylolpropane triacrylate: 6%,
[0150] Photoinitiator: 3%, specifically photoinitiator TPO is selected;
[0151] Leveling agent: 0.2%, specifically polydimethylsiloxane;
[0152] Solvent: 45.8%, specifically ethyl acetate.
[0153] In this application example, the preparation method of the smear-resistant coating is the same as that in [Application Example 1].
[0154]
Application example 4
[0155] A smear-resistant coating, which differs from [Application Example 2] in that:
[0156] The fluorosilicone modified acrylate resin is specifically selected from the fluorosilicone modified acrylate resin prepared in [Example 2].
[0157]
Application Example 5
[0158] A smear-resistant coating, which differs from [Application Example 2] in that:
[0159] The fluorosilicone modified acrylate resin is specifically selected from the fluorosilicone modified acrylate resin prepared in [Example 3].
[0160]
Application Example 6
[0161] A smear-resistant coating, which differs from [Application Example 2] in that:
[0162] The fluorosilicone modified acrylate resin is specifically selected from the fluorosilicone modified acrylate resin prepared in [Example 4].
[0163]
Application Example 7
[0164] A smear-resistant coating, which differs from [Application Example 2] in that:
[0165] The fluorosilicone modified acrylate resin is specifically selected from the fluorosilicone modified acrylate resin prepared in [Example 5].
[0166]
Application Example 8
[0167] A smear-resistant coating, which differs from [Application Example 2] in that:
[0168] The fluorosilicone modified acrylate resin is specifically selected from the fluorosilicone modified acrylate resin prepared in [Example 6].
[0169] Comparative Application Examples
[0170]
Comparative Application Example 1
[0171] A coating, which differs from [Application Example 2] in that:
[0172] The fluorosilicone modified acrylate resin is specifically selected from the fluorosilicone modified acrylate resin prepared in [Comparative Example 1].
[0173]
Comparative Application Example 2
[0174] A coating, which differs from [Application Example 2] in that:
[0175] The fluorosilicone modified acrylate resin is specifically selected from the fluorosilicone modified acrylate resin prepared in [Comparative Example 2].
[0176]
Comparative Application Example 3
[0177] A coating, which differs from [Application Example 2] in that:
[0178] The fluorosilicone modified acrylate resin is specifically selected from the fluorosilicone modified acrylate resin prepared in [Comparative Example 3].
[0179] Performance testing
[0180] Preparation of test samples:
[0181] The coatings prepared in Application Examples 1-8 and Comparative Application Examples 1-3 were coated on an ABS substrate by roller coating to a coating thickness of 10 μm, and then placed in a UV curing machine for light curing at an energy of 500 mJ / cm 2 , to obtain an ABS board with a cured coating layer.
[0182] (1) Wear resistance: The ABS plates cured with the coatings of different embodiments and comparative examples were left to stand for 48 hours, and then the wear resistance test was performed according to the wear resistance test method of Part 8 of GB / T4893.8-2013 Furniture Surface Paint Film Physical and Chemical Properties Test. The equipment was a paint film abrasion tester, the turntable speed was 60 r / min, and the test time was 100 min. The wear amount of the coating on the ABS plate was recorded. The smaller the wear amount, the better the wear resistance of the coating.
[0183] (2) Smear resistance:
[0184] 1. The ABS plates cured with coatings of different application examples and comparative application examples were left to stand for 48 hours, and then the stain resistance test was carried out according to the determination of stain resistance in Part 14 of GB / T3810.14-2016 Test Method for Ceramic Tiles, and the stain resistance level was recorded. The stain resistance level is divided into 1, 2, 3, 4, and 5 levels, and the higher the level, the more resistant the coating is to stain.
[0185] 2. After storing the ABS boards cured with coatings of different application examples and comparative application examples for 360 days, the stain resistance test was carried out in accordance with the determination of stain resistance in Part 14 of GB / T3810.14-2016 Test Method for Ceramic Tiles, and the stain resistance level was recorded.
[0186] 3. After the ABS plates coated with different application examples and comparative application examples were allowed to stand for 48 hours, they were boiled in 100°C water for 30 minutes, then taken out and allowed to stand for another 48 hours. Then, the stain resistance test was carried out in accordance with GB / T 3810.14-2016 Ceramic Tile Test Method Part 14 Determination of Stain Resistance, and the stain resistance level was recorded.
[0187] 4. According to GB / T 3810.14-2016 Ceramic Tile Test Method Part 14 Determination of Stain Resistance, perform a smear resistance test on the panels that have completed the wear resistance test in (1) and record the smear resistance level.
[0188] (3) Boiling resistance:
[0189] 1. The ABS plates of different application examples and comparative application examples were left to stand for 48 hours, and then the adhesion level of the coatings on the ABS plates of different application examples and comparative application examples was tested with tape according to the GB / T 9286-2021 paint and varnish cross-cut test method. The adhesion level is divided into 6 levels: 0, 1, 2, 3, 4, and 5. The lower the level, the better the adhesion stability of the coating.
[0190] 2. After the ABS plates of different application examples and comparative application examples were cured for 48 hours, they were boiled in 100°C water for 30 minutes, then taken out and allowed to stand for another 48 hours. Then, the adhesion grade of the paint film was tested according to the GB / T 9286-2021 paint and varnish cross-cut test method. The adhesion grade is divided into 6 grades: 0, 1, 2, 3, 4, and 5. The smaller the difference in grades, the better the high temperature resistance of the coating.
[0191] (4) Flexibility: Using tinplate as the substrate, the coatings in Application Example 1-8 and Comparative Application Example 1-3 were respectively coated on the substrate with a roller, and then placed in a UV curing machine for light curing. The energy used was 500 mJ / cm 2Finally, tinplates with different cured coatings were obtained, and the coating thickness was 5μm. After standing for 48 hours, the flexibility of the coating formed on the tinplate was tested in accordance with GB / T 1731-2020 Determination of flexibility of paint film and putty film, and the minimum shaft rod diameter at which no reticulation, cracks or peeling was observed was recorded.
[0192] Table 1 Coating performance test
[0193]
[0194] Comparative Application Examples 1-3 are compared with Application Example 7. In Comparative Application Example 1, the aliphatic polyurethane acrylate in the fluorosilicone modified acrylate resin is replaced by an equal amount of hydroxyethyl acrylate. Combined with the data in Table 1, it can be seen that after the aliphatic polyurethane acrylate is replaced by an equal amount of hydroxyethyl acrylate, the smear resistance of the coating is easily affected by storage time, high temperature and friction, and the long-term smear resistance of the coating changes significantly. At the same time, the flexibility of the coating is also reduced. Comparative Application Example 2 The styrene in the fluorosilicone modified acrylate resin is replaced by an equal amount of hexafunctional aliphatic polyurethane acrylate. Combined with the data in Table 1, it can be seen that after styrene is replaced by an equal amount of hexafunctional aliphatic polyurethane acrylate, the wear resistance and high temperature resistance of the coating change significantly. At the same time, the smear resistance of the coating is significantly affected by high temperature. In comparative application example 3, the carboxyl-containing acrylic monomer in the fluorosilicone-modified acrylate resin is replaced by an equal amount of hydroxyethyl acrylate. Combined with the data in Table 1, it can be seen that after the carboxyl-containing acrylic monomer is replaced by an equal amount of hydroxyethyl acrylate, the smear resistance of the coating is easily affected by storage time, high temperature and friction, and the long-term smear resistance of the coating changes significantly.
[0195] Combining Application Example 2 with Application Examples 4-8 and the data in Table 1, it can be seen that the fluorosilicone-modified acrylate resin for which protection is sought in this application can effectively improve the short-term smear resistance, long-term smear resistance, high temperature resistance, friction resistance and flexibility of the coating formed after the coating is cured, which is beneficial to extending the service life of the coating.
[0196] The difference between Application Example 8 and Application Example 7 is that in Application Example 8, the hydroxyl-containing acrylate monomer and the carboxyl-containing acrylate monomer are mixed in the preparation of the first monomer solution. Combined with the data in Table 1, it can be seen that the hydroxyl-containing acrylate monomer and the carboxyl-containing acrylic acid monomer are added when preparing the second monomer solution, which can further improve the coating's durable smear resistance.
[0197] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the specific implementation manner as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A fluorosilicone modified acrylate resin, characterized in that: The invention comprises the following raw materials in parts by weight: Styrene: 100-150 parts; Aliphatic polyurethane acrylate: 200-300 parts; Hydroxyl-containing acrylate monomer: 150-250 parts; Carboxyl-containing acrylic monomer: 20-50 parts; Fluorosilicone functional monomer: 50-150 parts; Initiator: 5-8 parts; Chain transfer agent: 1-3 parts; Alcohol solvent: 28-35 parts; Water: 5-12 parts; The fluorosilicone functional monomer is selected from any one of hexafluoropolyether trimethoxysilane and hexafluoropolyether triethoxysilane, or a combination of the two; Wherein, the structural formula of the hexacarbon perfluoropolyether trimethoxysilane is as follows: ; The structural formula of the hexacarbon perfluoropolyether triethoxysilane is as follows: ; The aliphatic polyurethane acrylate is selected from any one of tetrafunctional aliphatic polyurethane acrylate, pentafunctional aliphatic polyurethane acrylate, hexafunctional aliphatic polyurethane acrylate or a combination of several thereof; In addition, the preparation method of the fluorosilicone modified acrylate resin comprises the following steps: uniformly mixing an alcohol solvent with water to prepare a mixed solution; Add 30-50% of the total weight of the mixed solution to styrene, stir, and then continue to add aliphatic polyurethane acrylate, stir evenly, to obtain a first monomer solution; Adding hydroxyl-containing acrylate monomer, carboxyl-containing acrylic acid monomer and fluorosilicone functional monomer to the remaining mixed solution, heating to 40-50° C., reacting for 1-1.5 hours, to obtain a second monomer solution; The first monomer solution, the second monomer solution and the chain transfer agent are uniformly mixed, and then the initiator is added dropwise. The reaction temperature is controlled at 65-75° C. and the reaction is carried out for 2-4 hours to obtain a fluorosilicone modified acrylate resin.
2. A fluorosilicone modified acrylate resin according to claim 1, characterized in that: The hydroxyl-containing acrylate monomer is selected from any one of hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxyethyl acrylate, and hydroxypropyl acrylate, or a combination thereof; the carboxyl-containing acrylic acid monomer is selected from any one of acrylic acid and methacrylic acid, or a combination thereof.
3. The method for preparing a fluorosilicone modified acrylate resin according to any one of claims 1 to 2, characterized in that: The following steps are involved: The alcohol solvent is uniformly mixed with water to prepare a mixed solution; 30-50% of the total weight of the mixed solution is added to styrene, stirred, and then aliphatic polyurethane acrylate is added, stirred evenly, to obtain a first monomer solution; hydroxyl-containing acrylate monomer, carboxyl-containing acrylic monomer, and fluorosilicone functional monomer are added to the remaining mixed solution, the temperature is raised to 40-50°C, and the reaction is performed for 1-1.5 hours to obtain a second monomer solution; the first monomer solution, the second monomer solution, and the chain transfer agent are uniformly mixed, and then an initiator is added dropwise, the reaction temperature is controlled at 65-75°C, and the reaction is performed for 2-4 hours to obtain a fluorosilicone modified acrylate resin.
4. A smear-resistant coating, characterized in that: The method comprises the following raw materials in weight percentage: fluorosilicone modified acrylate resin: 35-45% trimethylolpropane triacrylate: 4-6% photoinitiator: 1-3% leveling aid: 0.1-0.2% solvent: balance; the fluorosilicone modified acrylate resin is the fluorosilicone modified acrylate resin according to any one of claims 1-2.
5. A graffiti-resistant coating according to claim 4, characterized in that: The photoinitiator is photoinitiator TPO.
6. A graffiti-resistant coating according to claim 4, characterized in that: The leveling agent is a silicone leveling agent, and the solvent is an alcohol or an ester.
7. A method for preparing a smear-resistant coating according to any one of claims 4 to 6, characterized in that: The following steps are involved: Uniformly dispersing fluorosilicone-modified acrylate resin, trimethylolpropane triacrylate and a photoinitiator in a solvent to obtain a dispersed solution; Add a leveling agent to the dispersed solution and stir evenly to obtain a smear-resistant coating.
Citation Information