A high-stiffness rubber pad and preparation method thereof

Through the preparation of modified polypropylene materials, the problems of insufficient toughness and wear resistance of rubber pads are solved, and high-stiffness rubber pads are prepared, which are suitable for special tire rubber with strong viscosity and have better performance than existing technologies.

CN117534905BActive Publication Date: 2024-10-11QINGDAO JIUSHAN COMPOSITE MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311535620.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-17
Publication Date
2024-10-11
Estimated Expiration
2043-11-17

AI Technical Summary

Technical Problem

Existing rubber pads made of polypropylene and polyethylene have problems such as poor toughness, unsatisfactory wear resistance, and insufficient stiffness during use, and cannot meet the needs of products with different rubber formulas.

Method used

Polypropylene modified material is used, consisting of PP, UHMWPE, fillers, modifiers, nucleating agents, coupling agents, antioxidants and lubricants, and is prepared with high stiffness through high-speed mixing, melt extrusion and stretching processes. rubber cloth.

Benefits of technology

The strength and toughness of the modified polypropylene material are significantly improved, and the stiffness and wear resistance of the rubber pad are improved, making it suitable for special tire rubber with strong viscosity, and its performance is better than the existing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004554887050000081
    Figure BDA0004554887050000081
  • Figure BDA0004554887050000091
    Figure BDA0004554887050000091
  • Figure BDA0004554887050000121
    Figure BDA0004554887050000121
Patent Text Reader

Abstract

The invention discloses a polypropylene modified material and a preparation method thereof, a high-stiffness rubber pad and a preparation method thereof. A polypropylene modified material is composed of the following raw materials in parts by weight: PP: 60-90 parts; UHMWPE: 10-40 parts; filler: 4-8 parts; modifier: 2-10 parts; nucleating agent: 0.1-1 parts; coupling agent: 0.5-4 parts; antioxidant: 0.1-0.5 parts; lubricant: 0.5-1 parts. A high-stiffness rubber pad is made from the above-mentioned polypropylene modified material as raw material. The stiffness and wear resistance of the rubber pad are better than those of the PP pad in the prior art. The pad surface of the rubber pad has a smaller contact area with the rubber, and the stiffness is higher. It is easier to peel the rubber from the rubber pad, and it is particularly suitable for special tire rubber with particularly strong viscosity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of rubber pads, and in particular to a high-stiffness rubber pad and a preparation method thereof. Background Art

[0002] In the production process from rubber to tire, first of all, the raw materials need to be mixed together according to the formula for banburying. After banburying, the mixed rubber needs to be transported to different places for preparation of materials for other processes, such as: bead assembly line, inner liner calendering line, steel belt calendering production line, cord calendering production line, sidewall extrusion production line, tread extrusion production line, etc. In other words, different rubber formulas are mixed with other raw materials (cords, steel wires, etc.) after the banburying process at other stations to complete the manufacture of different parts of the tire. Rubber mats are needed in the process of rubber transfer and storage. Rubber mats are used to transfer rubber or separate it into rolls for placement, which places high requirements on the heat resistance, toughness and stiffness of the rubber mats. The rubber mat materials commonly used in the prior art include polypropylene (PP), polyethylene (PE) and polyethylene terephthalate (PET), etc.

[0003] Polypropylene (PP) is a polymer made of propylene. It has the advantages of low density, high strength, corrosion resistance, and easy molding. However, PP has defects such as poor toughness, unsatisfactory wear resistance, and poor thermomechanical properties, which limit the scope of use of PP. In addition, the application effect of PP in rubber pads is not ideal, and the stiffness and wear resistance are not enough, resulting in a general service life. Polyethylene (PE) resin has high crystallinity, high density, good mechanical strength, high operating temperature, and good low temperature resistance. However, polyethylene products have the disadvantages of low hardness, poor toughness, poor load-bearing capacity, and poor resistance to environmental stress cracking.

[0004] Therefore, the rubber pad made of polypropylene or polyethylene cannot meet the use requirements of rubber products with various formulas, and the existing technology needs to be improved urgently. Summary of the invention

[0005] In order to solve the problems of poor toughness and unsatisfactory wear resistance of the above-mentioned PP material, insufficient stiffness and poor wear resistance in the application of rubber pads, the present invention provides a polypropylene modified material and a preparation method thereof, a high-stiffness rubber pad and a preparation method thereof.

[0006] In a first aspect, the present invention provides a polypropylene modified material, which is composed of the following raw materials in parts by weight: PP: 60-90 parts; UHMWPE: 10-40 parts; filler: 4-8 parts; modifier: 2-10 parts; nucleating agent: 0.1-1 part; coupling agent: 0.5-4 parts; antioxidant: 0.1-0.5 parts; lubricant: 0.5-1 parts.

[0007] Preferably, the polypropylene modified material is composed of the following raw materials in parts by weight: PP: 80-85 parts; UHMWPE: 15-20 parts; filler: 6-8 parts; modifier: 8-10 parts; nucleating agent: 0.5-1 parts; coupling agent: 3-3.5 parts; antioxidant: 0.5 parts; lubricant: 0.8 parts.

[0008] Optionally, the filler is any one of kaolin, calcium carbonate, glass fiber, and Nano-CaCO3; the preferred filler is Nano-CaCO3.

[0009] Preferably, the modifier is white oil.

[0010] Optionally, the nucleating agent is any one of an inorganic nucleating agent, an organic nucleating agent, a polymer nucleating agent, and a composite nucleating agent. The inorganic nucleating agent is any one of aluminosilicates, silicon dioxide, talcum powder, titanium dioxide, and calcium carbonate; the organic nucleating agent is any one of carboxylic acids and their salts, sorbitols, and organic phosphates; the polymer nucleating agent is any one of vinyl cyclohexane and vinyl cyclopentane. The nucleating agent can promote the uniform and refined crystallization of polyethylene and ensure mechanical properties. The preferred nucleating agent is halloysite nanotubes (HNTs) of aluminosilicates. Halloysite nanotubes can enhance the mechanical properties of polymers such as strength, stiffness, and heat resistance due to their tubular structure and high specific surface area.

[0011] Optionally, the coupling agent is any one of a silane coupling agent, a titanate coupling agent, and polyethylene grafted maleic anhydride. The preferred coupling agent is vinyl trimethoxy silane.

[0012] Preferably, the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:2.5. Highly effective antioxidants can ensure that the present invention does not degrade during processing.

[0013] Preferably, the lubricant is polyethylene wax.

[0014] In a second aspect, the present invention provides a method for preparing a polypropylene modified material, the preparation method comprising the following steps:

[0015] S1: Mixing the PP, UHMWPE, filler and modifier in the formula in a high-speed mixer at a high speed at a mixing temperature of 50 to 80° C. and sieving to obtain a mixture 1;

[0016] S2: feeding the mixture 1 obtained in S1 into a melt extruder for mixing to obtain a mixture 2;

[0017] S3: adding the formulated amount of nucleating agent, coupling agent, antioxidant and lubricant to the mixture 2 obtained in S2 and continuing to mix;

[0018] S4: After S3 is evenly mixed, the temperature is lowered and cooled to obtain the polypropylene modified material.

[0019] Furthermore, the temperature of the melt extruder in step S2 is 190-240° C.; the screw speed of the melt extruder in step S2 is 460-520 rpm.

[0020] In a third aspect, the above-mentioned modified polypropylene material is used in the preparation of rubber pads, rubber fibers or rubber films.

[0021] In the fourth aspect, based on the same invention of the above-mentioned polypropylene modified material, the present invention also provides a high-stiffness rubber pad cloth prepared using the polypropylene modified material obtained in the first aspect and the second aspect.

[0022] In a fifth aspect, the present invention further provides a method for preparing the high-stiffness rubber pad cloth described in the fourth aspect, the preparation method is as follows:

[0023] S1: Using polypropylene modified material particles as the base material,

[0024] S2: hot-melt extrusion and spinning of the polypropylene modified material particles to obtain polypropylene modified fibers;

[0025] S3: sending the modified polypropylene yarn into a stretching machine for stretching treatment;

[0026] S4: doubling, twisting, warping and drawing the polypropylene modified yarn obtained in S3;

[0027] S5: then the cloth is sent to a loom for weaving;

[0028] S6: shaping and slitting the woven fabric obtained in S5 to obtain a high-stiffness polypropylene modified rubber pad;

[0029] S7: Performing quality inspection on the obtained polypropylene modified rubber pad.

[0030] Furthermore, the cross section of the modified polypropylene yarn obtained in S2 is circular or hexagonal; the specification of the high-stiffness rubber pad cloth obtained in S6 is 680D / 60F.

[0031] Compared with the prior art, the present invention has the following advantages:

[0032] 1. The present invention provides a polypropylene modified material and a preparation method thereof. The strength and toughness of the prepared polypropylene modified material are significantly better than those of existing polypropylene materials. The present invention utilizes the excellent impact resistance and wear resistance of UHMWPE to blend with PP to improve the toughness of PP, and the strength decrease is not obvious. UHMWPE crystals aggregate and the molecular chains are interconnected to form a complex network continuous structure, so the impact performance of PP can be improved. White oil is used to solve the problem of high entanglement of UHMWPE molecular chains, and the strength and toughness of the obtained polypropylene modified material are significantly better than those of existing polypropylene materials.

[0033] 2. The present invention provides a rubber pad made of the above-mentioned polypropylene material, and the stiffness and wear resistance of the rubber pad are better than those of the PP pad in the prior art.

[0034] 3. The rubber pad preparation method of the present invention changes the circular cross-section of the polypropylene filaments in the prior art into a hexagonal shape, thereby increasing the lateral friction of the polypropylene filaments, making the contact area between the pad surface and the rubber of the rubber pad smaller, and making the stiffness higher. It is easier to peel the rubber from the rubber pad, and is particularly suitable for special tire rubbers with particularly strong viscosity. DETAILED DESCRIPTION

[0035] The technical scheme of the present invention will be clearly and completely described below in conjunction with embodiments and experimental data. Obviously, the described embodiments are only a part of embodiments of the present invention, rather than all embodiments. Based on the embodiments in the present invention, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention. In the present invention, unless otherwise specified, the equipment and raw materials used, etc. can be purchased from the market or are commonly used in this area. The methods in the following embodiments, if not otherwise specified, are conventional methods in this area. It should be understood that, if not otherwise specified, the various raw materials in the present invention can be obtained commercially.

[0036] Embodiment 1:

[0037] A polypropylene modified material is composed of the following raw materials in parts by weight:

[0038] PP: 85 parts; UHMWPE: 15 parts; filler: 6 parts; modifier: 10 parts; nucleating agent: 0.8 parts; coupling agent: 3.5 parts; antioxidant: 0.5 parts; lubricant: 0.8 parts.

[0039] In this embodiment, the filler is Nano-CaCO3; the modifier is white oil; the nucleating agent is an inorganic nucleating agent, the inorganic nucleating agent is aluminosilicate, and the aluminosilicate nucleating agent is specifically halloysite nanotubes (HNTs); the coupling agent is a silane coupling agent, and the silane coupling agent is specifically vinyltrimethoxysilane; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:2.5; the lubricant is polyethylene wax.

[0040] Preparation method: Prepare the materials according to the composition ratio of the raw materials in this embodiment;

[0041] S1: Mixing the PP, UHMWPE, filler and modifier in the formula in a high-speed mixer at a high speed at a mixing temperature of 50 to 80° C. and sieving to obtain a mixture 1;

[0042] S2: feeding the mixture 1 obtained in S1 into a melt extruder for mixing to obtain a mixture 2;

[0043] S3: adding the formulated amount of nucleating agent, coupling agent, antioxidant and lubricant to the mixture 2 obtained in S2 and continuing to mix;

[0044] S4: After S3 is evenly mixed, the temperature is lowered and cooled to obtain the polypropylene modified material.

[0045] The temperature of the melt extruder in step S2 is 190-240° C.; the screw speed of the melt extruder in step S2 is 460-520 rpm.

[0046] Embodiment 2:

[0047] A polypropylene modified material is composed of the following raw materials in parts by weight:

[0048] PP: 80 parts; UHMWPE: 20 parts; filler: 8 parts; modifier: 10 parts; nucleating agent: 0.8 parts; coupling agent: 3 parts; antioxidant: 0.5 parts; lubricant: 0.8 parts.

[0049] In this embodiment, the filler is Nano-CaCO3; the modifier is white oil; the nucleating agent is an inorganic nucleating agent, the inorganic nucleating agent is aluminosilicate, and the aluminosilicate nucleating agent is specifically halloysite nanotubes (HNTs); the coupling agent is a titanate coupling agent, and the titanate coupling agent is specifically triisostearyl titanate isopropyl ester (TTS); the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:2.5; the lubricant is polyethylene wax.

[0050] The preparation method is the same as Example 1.

[0051] Embodiment 3:

[0052] A polypropylene modified material is composed of the following raw materials in parts by weight:

[0053] PP: 85 parts; UHMWPE: 15 parts; filler: 6 parts; modifier: 8 parts; nucleating agent: 1 part; coupling agent: 3.5 parts; antioxidant: 0.5 parts; lubricant: 0.8 parts.

[0054] In this embodiment, the filler is calcium carbonate; the modifier is white oil; the nucleating agent is an organic nucleating agent, and the organic nucleating agent is an organic phosphate; the coupling agent is a silane coupling agent, and the silane coupling agent is specifically vinyltrimethoxysilane; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:2.5; and the lubricant is polyethylene wax.

[0055] The preparation method is the same as Example 1.

[0056] Embodiment 4:

[0057] A polypropylene modified material is composed of the following raw materials in parts by weight:

[0058] PP: 80 parts; UHMWPE: 20 parts; filler: 6 parts; modifier: 8 parts; nucleating agent: 1 part; coupling agent: 3 parts; antioxidant: 0.5 parts; lubricant: 0.8 parts.

[0059] In this embodiment, the filler is calcium carbonate; the modifier is white oil; the nucleating agent is an organic nucleating agent, and the organic nucleating agent is an organic phosphate; the coupling agent is a titanate coupling agent, and the titanate coupling agent is specifically triisostearyl titanate isopropyl ester (TTS); the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:2.5; and the lubricant is polyethylene wax.

[0060] The preparation method is the same as Example 1.

[0061] Embodiment 5:

[0062] A polypropylene modified material is composed of the following raw materials in parts by weight:

[0063] PP: 85 parts; UHMWPE: 15 parts; filler: 6 parts; modifier: 10 parts; nucleating agent: 0.5 parts; coupling agent: 3.5 parts; antioxidant: 0.5 parts; lubricant: 0.8 parts.

[0064] In this embodiment, the filler is Nano-CaCO3; the modifier is white oil; the nucleating agent is a polymer nucleating agent, and the polymer nucleating agent is specifically vinyl cyclohexane; the coupling agent is a silane coupling agent, and the silane coupling agent is specifically vinyl trimethoxy silane; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:2.5; and the lubricant is polyethylene wax.

[0065] The preparation method is the same as Example 1.

[0066] Embodiment 6:

[0067] A polypropylene modified material is composed of the following raw materials in parts by weight:

[0068] PP: 80 parts; UHMWPE: 20 parts; filler: 8 parts; modifier: 10 parts; nucleating agent: 0.5 parts; coupling agent: 3 parts; antioxidant: 0.5 parts; lubricant: 0.8 parts.

[0069] In this embodiment, the filler is Nano-CaCO3; the modifier is white oil; the nucleating agent is a polymer nucleating agent, and the polymer nucleating agent is specifically vinyl cyclohexane; the coupling agent is a titanate coupling agent, and the titanate coupling agent is specifically triisostearyl titanate isopropyl ester (TTS); the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:2.5; and the lubricant is polyethylene wax.

[0070] The preparation method is the same as Example 1.

[0071] Comparative Example 1:

[0072] Commercially available conventional polypropylene (PP) material.

[0073] Comparative Example 2:

[0074] Commercially available conventional polyethylene (PE) materials.

[0075] Experimental analysis of Examples 1-6 and Comparative Examples 1-2:

[0076] The test indicators and test methods are as follows:

[0077] Density, the testing method is: GB / T 40006.3-2021; tensile strength, the testing method is: GB / T1040-2006; notched impact strength, the testing method is: GB / T1843-2008.

[0078] The specific test results of Examples 1-6 and Comparative Examples 1-2 are shown in Table 1:

[0079] Table 1 Polypropylene modification test results of Examples 1-6 and Comparative Examples 1-2

[0080]

[0081]

[0082] In theory, UHMWPE is a special polyethylene with excellent impact resistance, wear resistance, etc. UHMWPE can improve the toughness of PP, and the strength decrease is not obvious. Due to the aggregation of UHMWPE crystals and the interconnection between molecular chains, a complex network continuous structure is formed, so the impact performance of PP can be improved. However, due to the high entanglement of UHMWPE molecular chains, the melt viscosity of UHMWPE is large, and the huge viscosity mismatch between the blend components inhibits the hybrid dynamics of the polymer melt, resulting in poor blending effect and deterioration of the performance of PP / UHMWPE blends.

[0083] The present invention adopts white oil to improve the dispersion and flow properties of UHMWPE in the matrix and promote the dispersion of UHMWPE in the PP matrix; the above-mentioned defects of the prior art are overcome, and in addition, the introduction of an appropriate amount of Nano-CaCO3 into the blending system can effectively improve the comprehensive performance of the system and improve the strength and toughness of the material.

[0084] From the comparison of the above experimental results in Table 1, it can be seen that the performance of Examples 1-6 is significantly better than that of Comparative Examples 1-2, especially Example 1 has the best performance, and the density, tensile strength and impact strength are significantly improved; in addition, the 6 embodiment schemes provided by the present invention improve the tensile strength of the polypropylene modified material while improving its impact strength, thereby obtaining a PP modified material with excellent comprehensive performance.

[0085] Embodiment 7:

[0086] Based on the polypropylene modified material obtained by the best formula of the above embodiment 1, a high stiffness rubber pad is prepared using it as a raw material, and the preparation method thereof is as follows:

[0087] S1: Using polypropylene modified material particles as the base material,

[0088] S2: hot-melt extrusion and spinning of the polypropylene modified material particles to obtain polypropylene modified fibers;

[0089] S3: sending the modified polypropylene yarn into a stretching machine for stretching treatment;

[0090] S4: doubling, twisting, warping and drawing-in of the polypropylene modified yarn obtained in S3;

[0091] S5: then the cloth is sent to a loom for weaving;

[0092] S6: shaping and cutting the woven fabric obtained in S5 to obtain a high-performance polypropylene modified rubber pad;

[0093] S7: Performing quality inspection on the obtained polypropylene modified rubber pad.

[0094] Furthermore, the cross section of the modified polypropylene yarn obtained in S2 is hexagonal, and the specification of the high-stiffness rubber pad cloth obtained in S6 is 680D / 60F.

[0095] Embodiment 8:

[0096] Compared with Example 7, the difference is that the cross-section of the polypropylene modified yarn obtained in S2 is hexagonal, and the specification of the high-stiffness rubber pad cloth obtained in S6 is 600D / 122F.

[0097] Embodiment 9:

[0098] Compared with Example 7, the difference is that the cross-section of the polypropylene modified yarn obtained in S2 is circular, and the specification of the high-stiffness rubber pad cloth obtained in S6 is 680D / 60F.

[0099] Embodiment 10:

[0100] Compared with Example 7, the difference is that the cross-section of the polypropylene modified yarn obtained in S2 is circular, and the specification of the high-stiffness rubber pad cloth obtained in S6 is 600D / 122F.

[0101] Comparative Example 3:

[0102] A rubber pad is prepared using commercially available conventional polypropylene (PP) material as raw material, and the preparation method thereof is as follows:

[0103] S1: Use commercially available conventional polypropylene particles as the base material.

[0104] S2: hot-melt extrusion of commercially available conventional polypropylene material particles to obtain polypropylene filaments;

[0105] S3: feeding the polypropylene filament into a stretching machine for stretching treatment;

[0106] S4: doubling, twisting, warping and drawing in the polypropylene yarn obtained in S3;

[0107] S5: then the cloth is sent to a loom for weaving;

[0108] S6: shaping and cutting the woven fabric obtained in S5 to obtain a polypropylene rubber pad;

[0109] S7: Perform quality inspection on the obtained polypropylene rubber pad.

[0110] Furthermore, the cross section of the polypropylene filament obtained in S2 is circular, and the specification of the polypropylene rubber pad cloth obtained in S6 is 600D / 122F.

[0111] Comparative Example 4:

[0112] A rubber mat is prepared using commercially available conventional polyethylene (PE) material as raw material, and the preparation method thereof is as follows:

[0113] S1: Use commercially available conventional polyethylene material particles as the base material.

[0114] S2: hot-melt extrusion of commercially available conventional polyethylene material particles to obtain polyethylene filaments;

[0115] S3: sending the polyethylene filament into a stretching machine for stretching treatment;

[0116] S4: doubling, twisting, warping and drawing-in of the polyethylene yarn obtained in S3;

[0117] S5: then the cloth is sent to a loom for weaving;

[0118] S6: shaping and cutting the woven fabric obtained in S5 to obtain a polyethylene rubber pad;

[0119] S7: Perform quality inspection on the obtained polyethylene rubber pad.

[0120] Furthermore, the cross-section of the polyethylene filament obtained in S2 is circular, and the specification of the polyethylene rubber pad cloth obtained in S6 is 600D / 122F.

[0121] The specific test results of Examples 7-10 and Comparative Examples 3-4 are shown in Table 2:

[0122] Table 2 Rubber mat performance test results of Examples 7-10 and Comparative Examples 3-4

[0123]

[0124] From the comparison of the above experimental results in Table 2, it can be seen that the performance of the rubber pads of Examples 7-10 is significantly better than that of Comparative Examples 3 and 4. Compared with Examples 7-10, the rubber pad of Example 7 has the best performance, and its tensile strength, elongation and stiffness are significantly optimized and improved.

[0125] In summary, the rubber pad prepared from the polypropylene modified material provided by the present invention overcomes the shortcomings of the prior art. The rubber pad prepared from the polypropylene modified material has high stiffness and better tensile strength. The high-stiffness rubber pad is more suitable for special rubbers with strong viscosity.

[0126] It is understandable that those skilled in the art can make equivalent substitutions or changes based on the technical solution and concept of the present invention, and all these changes or substitutions should fall within the protection scope of the claims attached to the present invention.

Claims

1. A polypropylene modified material, characterized in that: It is composed of the following raw materials in parts by weight: PP: 85 parts; UHMWPE: 15 parts; filler: 6 parts; modifier: 10 parts; nucleating agent: 0.8 parts; coupling agent: 3.5 parts; antioxidant: 0.5 parts; lubricant: 0.8 parts; The filler is Nano-CaCO3; the modifier is white oil; the nucleating agent is an inorganic nucleating agent, the inorganic nucleating agent is aluminosilicate, and the aluminosilicate nucleating agent is specifically halloysite nanotubes (HNTs); the coupling agent is a silane coupling agent, and the silane coupling agent is specifically vinyl trimethoxy silane; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:2.5; the lubricant is polyethylene wax; The preparation method of the polypropylene modified material is characterized in that the preparation method comprises the following steps: S1: Mix the PP, UHMWPE, filler and modifier in the formula in a high-speed mixer at a high speed at a mixing temperature of 50-80°C, and sieve to obtain a mixture 1; S2: feeding the mixture 1 obtained in S1 into a melt extruder for mixing to obtain a mixture 2; S3: adding the formulated amount of nucleating agent, coupling agent, antioxidant and lubricant to the mixture 2 obtained in S2 and continuing to mix; S4: After S3 is evenly mixed, the temperature is lowered and cooled to obtain the polypropylene modified material.

2. A polypropylene modified material according to claim 1, characterized in that: The temperature of the melt extruder in step S2 is 190-240° C.; the screw speed of the melt extruder in step S2 is 460-520 rpm.

3. Use of the modified polypropylene material according to claim 1 in the preparation of rubber pads, rubber fibers or rubber films.

4. A high stiffness rubber pad, characterized in that: The raw material for preparing the rubber pad is the polypropylene modified material described in claim 1.

5. The rubber pad according to claim 4, characterized in that: The preparation method of the rubber pad is as follows: S1: Using polypropylene modified material particles as the base material, S2: hot-melt extrusion and spinning of the polypropylene modified material particles to obtain polypropylene modified fibers; S3: sending the modified polypropylene yarn into a stretching machine for stretching treatment; S4: doubling, twisting, warping and drawing-in of the polypropylene modified yarn obtained in S3; S5: then the cloth is sent to a loom for weaving; S6: shaping and cutting the woven fabric obtained in S5 to obtain a high-performance polypropylene modified rubber pad; S7: Performing quality inspection on the obtained polypropylene modified rubber pad; The cross section of the modified polypropylene yarn obtained in S2 is circular or hexagonal; the specification of the high-stiffness rubber pad cloth obtained in S6 is 680D / 60F.