Preparation and application of high-efficiency super-stable oxygen evolution catalyst wn-nife ldh with zipper tooth interlocking structure

By constructing a WN-NiFe LDH catalyst with a zipper-like interlocking structure, the problem of poor stability of NiFe-LDH-based catalysts in OER was solved, achieving efficient and stable oxygen evolution performance, which has commercial application potential.

CN117535720BActive Publication Date: 2026-11-10BEIJING UNIV OF CHEM TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311367574.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-22
Publication Date
2026-11-10
Estimated Expiration
2043-10-22

AI Technical Summary

Technical Problem

Existing NiFe-LDH-based catalysts suffer from poor stability, lack of active edge sites, slow proton diffusion, and easy deactivation in the oxygen evolution reaction (OER), which limits their commercial application.

Method used

A WN-NiFe LDH catalyst with a zipper-like interlocking structure was constructed. Zipper-like WN was prepared by hydrothermal method, and the interlocking structure of WN-NiFe LDH was formed by electrochemical deposition, which enhanced the stability and activity of the catalyst.

Benefits of technology

It significantly improves the stability and activity of the catalyst, with an order-of-magnitude increase in stability, avoids catalyst deactivation, and exhibits excellent oxygen evolution performance, showing potential for commercial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004504969220000081
    Figure BDA0004504969220000081
  • Figure BDA0004504969220000091
    Figure BDA0004504969220000091
  • Figure HDA0004504969230000011
    Figure HDA0004504969230000011
Patent Text Reader

Abstract

The preparation and application of WN-NiFe LDH, a highly efficient and ultra-stable oxygen evolution catalyst with a zipper-like interlocking structure, belong to the field of oxygen evolution catalysts. First, WN with a zipper-like structure is prepared. Using WN as a precursor, the final highly efficient and stable oxygen evolution catalyst WN-NiFe LDH with a zipper-like interlocking structure is prepared by electrochemical deposition. Ni and Fe ions in solution are deposited on the precursor using electrochemical deposition, promoting the coupling between the precursor and the layered metal compound, resulting in the final highly efficient and stable oxygen evolution catalyst WN-NiFe LDH with a zipper-like interlocking structure. This interlocking structure not only improves the OER performance of nickel-iron-based catalysts but also greatly enhances OER stability by slowing catalyst dissolution, promoting catalyst phase transformation, mitigating passivation, and accelerating bubble release.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of water electrolysis technology, and in particular to a method for preparing and applying a highly efficient and ultra-stable oxygen evolution catalyst, WN-NiFe LDH, with a zipper-like interlocking structure. Background Technology

[0002] Water splitting to produce hydrogen and oxygen is considered one of the most promising methods to alleviate the energy crisis and environmental degradation, encompassing two half-reactions: the hydrogen evolution reaction (HER) and the oxygen evolution reaction (OER). Due to the slow kinetics of the multi-step four-electron OER process, it still requires a larger overpotential to drive OER compared to HER, even when using noble metal Ru-based or Ir-based catalysts. However, the high cost, low abundance, and poor stability of noble metal catalysts severely limit their commercial application. Therefore, discovering high-performance non-noble metal (NPM) catalysts for OER is an extremely important issue.

[0003] Recent reports on the excellent catalytic activity of NiFe-based catalysts in OER reactions under high voltages suggest they may replace expensive noble metal catalysts. Among these, NiFe-LDH is considered to be a Fe... 3+ Doped Ni(OH)₂. Due to the typical layered structure of NiFe-LDH, its performance can be improved over a wide range by adjusting the Ni to Fe ratio, the type of interlayer anions, and the porosity. These characteristics make NiFe-LDH a promising material for energy conversion and storage.

[0004] Unfortunately, a systematic review of recent research findings on NiFe-LDH-based catalysts reveals that their efficient utilization is limited by their aggregation tendency, lack of active edge sites, and poor conductivity and stability. Specifically, in investigating the stability of NiFe-based bilayer hydroxides, it was found that proton acceptors (such as OH-) in the OER process... - The slow diffusion between NiFe-LDH layers leads to NiFe-LDH dissolution, resulting in poor stability during the reaction. Furthermore, various mechanisms such as crystal phase transformation, passivation, and bubble blockage can cause catalyst deactivation, indicating significant room for improvement in the stability of NiFe-LDH-based catalysts. This invention, by constructing a heterostructure that combines WN and NiFe-LDH using a zipper-like interlocking structure, successfully prepared a highly stable and high-performance oxygen evolution catalyst, WN-NiFe LDH. This effectively avoids these deactivation mechanisms, resulting in an order-of-magnitude improvement in stability at a fixed current density compared to traditional NiFe LDH, potentially enabling commercial applications. Summary of the Invention

[0005] The purpose of this invention is to provide a WN-NiFe LDH oxygen evolution catalyst with a zipper-like interlocking structure, its preparation method and application. The preparation method is simple, it has excellent oxygen evolution performance, and more importantly, its stability is improved by orders of magnitude compared with the OER reference catalysts RuO2 and NiFe LDH, which is expected to realize large-scale application.

[0006] To achieve the above-mentioned objectives, the present invention provides the following technical solution:

[0007] This invention provides a method for preparing a WN-NiFe LDH oxygen evolution catalyst with a zipper-like interlocking structure, comprising the following steps:

[0008] Step (1): Zipper tooth-shaped WO3 is prepared using a hydrothermal method with a tungsten source. The zipper tooth-shaped WO3 is mixed with nitrogen-containing substances in a certain proportion and calcined at high temperature to obtain WN with the same zipper tooth shape.

[0009] Step (2): Using the zipper-shaped WN prepared in step (1) as a precursor, the final WN-NiFe LDH oxygen evolution catalyst with a zipper-shaped interlocking structure is prepared by electrochemical deposition: First, a certain proportion of Ni source and Fe source are dissolved in deionized water and mixed evenly by ultrasound and stirring to form solution A; then a certain amount of solution A is poured into the electrodeposition tank, and Ni ions and Fe ions in the solution are deposited on the zipper-shaped WN precursor by electrochemical deposition, so as to promote the formation of an interlocking structure between the zipper-shaped WN precursor and the layered NiFe metal compound, and finally obtain the highly efficient and stable oxygen evolution catalyst WN-NiFe LDH with a zipper-shaped interlocking structure.

[0010] Preferably, in step (1) the preparation of zipper tooth-shaped WO3: for every 1.5 mmol Na2WO4·H2O, there are 4.2 mmol H2C2O4, 1.15 mmol H8N2O8S2, and 30 mL of deionized water. After dissolution, hydrochloric acid is slowly and continuously added to adjust the pH to 1-5. After mixing evenly, purified carbon cloth (CC) is added and reacted at 100-250℃ for 5-20 h. The mixture is then dried under a nitrogen atmosphere to obtain zipper tooth-shaped WO3.

[0011] Preferably, step (1): the zipper-shaped WO3 obtained above is placed downstream of the tubular furnace.

[0012] A nitrogen source is placed upstream, and sintering at 600-1000℃ for 1-5 hours yields zipper-tooth-shaped WN. The nitrogen source is melamine, dicyandiamide, urea, etc.; the mass ratio of nitrogen source to WO3 is 1:2 to 50:1. Further, following the matching principles of temperature, time, and melamine, the WO3 is nitrided into zipper-tooth-shaped WN.

[0013] Preferably, step (2) involves electrochemical deposition using the zipper-tooth WN prepared in step (1) as the current collector. A certain proportion of Ni and Fe sources are dissolved in deionized water and mixed uniformly using ultrasound and stirring to form solution A. The zipper-tooth WN is used as the working electrode, with a graphite rod and Ag / AgCl serving as the counter and reference electrodes, respectively. Electrochemical deposition is performed using a chronoamperometric method at a voltage of -5V to 5V for a deposition time of 300s to 2000s. The WN-NiFe LDH with a zipper-tooth interlocking structure is obtained after drying under a nitrogen atmosphere.

[0014] The molar concentration of nickel source in solution A is 5 mM to 50 mM, and the molar concentration of iron source is 5 mM to 50 mM.

[0015] The present invention provides a method for preparing a WN-NiFe LDH high-efficiency and stable oxygen evolution catalyst with a zipper-like interlocking structure by the preparation method described above.

[0016] In the catalyst obtained by this invention, the WN surface has a serrated structure on one side of a zipper, and the NiFe metal layered compound NiFe LDH surface also has a serrated structure. The teeth on the WN surface and the teeth on the NiFe LDH surface mesh to form a heterojunction with zipper-like interlocking. Two WNs are interlocked on each side of a NiFe LDH via serrated meshing, thus forming a zipper-like interlocking structure, i.e., two WNs are interlocked and connected by a NiFe LDH in the middle.

[0017] The stability of the obtained catalyst is maintained at a current density of 10 mA cm⁻¹ -2 ~100mA cm -2 The duration should not be less than 1000 hours.

[0018] At 50mA cm -2 In stability tests, Fe segregation in WN-NiFe LDH was much smaller than in NiFe LDH; the bubble contact angle of WN-NiFeLDH in water was 148.10°; and at room temperature (25°C) and a fixed current density of 50 mA / cm², the stability was achieved. -2 Under 1M KOH electrolyte conditions, after more than 1000 hours, the overpotential increased by only 35mV, the LSV change was negligible, and the element type and distribution had negligible effects. Furthermore, WN-NiFe LDH showed negligible effects at high current densities (>300mA cm⁻¹). -2 It also exhibits excellent stability, continuously emitting oxygen for over 500 hours.

[0019] This invention provides the application of the WN-NiFe LDH oxygen evolution catalyst with zipper-like interlocking structure described above in water electrolysis. Thanks to the mutual restriction between WN and NiFe LDH, Fe segregation is effectively reduced, catalyst passivation is prevented, bubble blockage is avoided, and the oxygen evolution catalytic performance and catalyst life are significantly increased.

[0020] This invention provides a method for preparing a WN-NiFe LDH oxygen evolution catalyst with a zipper-like interlocking structure. Through the effective interlocking effect between WN and NiFe LDH, Fe segregation can be effectively avoided; proton acceptor migration is accelerated, enabling faster conversion into active material; passivation of the catalyst during the reaction process is effectively avoided; and catalyst deactivation due to electrode blockage is effectively prevented by rapidly releasing gas from the catalyst surface. Not only does it exhibit excellent oxygen evolution performance, but more importantly, its catalytic stability is improved by orders of magnitude compared to the traditional commercial oxygen evolution catalyst RuO2. This work provides new insights into the design and preparation of highly efficient and stable catalysts, not only for OER catalysts. Attached Figure Description

[0021] Figure 1 This is a schematic diagram of the synthesis method in Example 1;

[0022] Figure 2 The XRD pattern of WO3, the intermediate in Example 1;

[0023] Figure 3 Here is the SEM image of WO3, the intermediate in Example 1;

[0024] Figure 4 This is the XRD pattern for Comparative Example 1;

[0025] Figure 5 This is the XRD pattern for Comparative Example 2;

[0026] Figure 6 Here is the XRD pattern for Example 1;

[0027] Figure 7 The images shown are the SEM image, TEM image, and elemental mapping diagram of Comparative Example 1.

[0028] Figure 8 The images shown are the SEM images, TEM images, and elemental mapping diagrams for Comparative Example 2.

[0029] Figure 9 The SEM image, TEM image, and elemental mapping image are for Example 1.

[0030] Figure 10 X-ray photoelectron spectroscopy (XPS) for Example 1, Comparative Example 1, and Comparative Example 2;

[0031] Figure 11 A comparison chart of the oxygen evolution performance of Example 1 and Example 2 after iR correction;

[0032] Figure 12 A comparison chart of oxygen evolution performance after iR correction for Examples 1, 3 and 4;

[0033] Figure 13 Comparison of oxygen evolution performance between Example 1, Comparative Examples 1-2 and commercial RuO2 and CC after iR correction;

[0034] Figure 14 This is a timing voltage test diagram for Comparative Example 1;

[0035] Figure 15 Comparison charts of Example 1, Comparative Example 2, and commercial RuO2 timing voltage tests;

[0036] Figure 16 The graph shows a comparison between the initial LSV curve of Example 1 and the oxygen evolution performance after stability testing without iR correction.

[0037] Figure 17 The TEM image and elemental mapping diagram are shown after the stability test of Example 1.

[0038] Figure 18 The in-situ Raman spectrum of Example 1;

[0039] Figure 19 The in-situ Raman spectrum of Comparative Example 2;

[0040] Figure 20 The uncorrected CV curves for Example 1 and Comparative Example 2 are shown.

[0041] Figure 21 The amount of Fe segregation during the stability test of Example 1 and Comparative Example 2;

[0042] Figure 22 The bubble contact angles under liquid in Example 1 and Comparative Example 2 are shown.

[0043] Figure 23 Example 1 shows the effect at high current density (>300mA cm⁻¹). -2 The timing current density test diagram. Detailed Implementation

[0044] This invention provides a method for preparing a WN-NiFe LDH oxygen evolution catalyst with a zipper-like interlocking structure, comprising the following steps:

[0045] In this invention, unless otherwise specified, all raw materials required for preparation are commercially available products well known to those skilled in the art.

[0046] This invention provides the application of the highly stable oxygen evolution catalyst WN-NiFe LDH described in the above technical solution in water electrolysis. This invention does not specifically limit the method of application; any method well-known in the art can be used.

[0047] The present invention will be further illustrated below with specific examples. The described embodiments are merely some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

[0048] Example 1:

[0049] In step (1), 1.5 mmol sodium tungstate, 4.2 mmol oxalic acid, and 1.15 mmol ammonium persulfate were dissolved in 30 ml of deionized water, and the pH was adjusted to approximately 1.2 with hydrochloric acid of appropriate concentration. The mixture was then reacted at 180 °C to obtain zipper-tooth-shaped WO3 loaded onto carbon cloth. Then, 350 mg of melamine was added to a tube furnace, and the mixture was sintered at 800 °C for 2 h under an argon atmosphere to obtain WN with the same zipper-tooth-like structure.

[0050] Step (2): Using the WN obtained in step (1) as the current collector, the metal salts of nickel nitrate and iron nitrate are electrodeposited for 600s using the chronoamperometry at a voltage of -5V to 5V to obtain WN-NiFe LDH with a zipper-like interlocking heterostructure, named WN(-800℃)-NiFe LDH(-600s).

[0051] Example 2:

[0052] Except for changing the sintering temperature to 900℃, the other implementation methods are the same as in Example 1, resulting in WN-NiFe LDH with a zipper-like interlocking heterostructure, named WN-900℃-NiFe LDH-600s.

[0053] Example 3:

[0054] Except for changing the electrodeposition time to 900s, the other implementation methods are the same as in Example 1, resulting in WN-NiFe LDH with a zipper-like interlocking heterostructure, named WN-800℃-NiFe LDH-900s.

[0055] Example 4:

[0056] Except for changing the electrodeposition time to 1200s, the other implementation methods are the same as in Example 1, resulting in WN-NiFe LDH with a zipper-like interlocking heterostructure, named WN-800℃-NiFe LDH-1200s.

[0057] Comparative Example 1:

[0058] Zipper-shaped WNs were prepared using the same method as in Example 1, but without the electrodeposition step.

[0059] Comparative Example 2:

[0060] Without preparing WN, NiFe LDH was prepared directly on carbon cloth by electrodeposition using the same method as in Example 1.

[0061] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

[0062] Materials characterization and testing

[0063] Figure 1 The preparation process of a high-performance and high-stability WN-NiFe LDH catalyst with a zipper-like interlocking structure;

[0064] Figure 2 This demonstrates that the intermediate WO3 was successfully prepared using this method.

[0065] Figure 3 Note that the WO3 prepared by this method has a zipper-like structure;

[0066] Figure 4 This demonstrates the successful preparation of zipper-shaped WN in Comparative Example 1.

[0067] Figure 5 This indicates that Comparative Example 2, prepared by this electrodeposition method, has poor crystallinity and does not exhibit obvious XRD diffraction peaks.

[0068] Figure 6 Note that in Example 1, the XRD pattern of WN-NiFe LDH is consistent with that of WN, further proving... Figure 4 As mentioned, the NiFe LDH obtained by electrodeposition did not show obvious XRD diffraction peaks due to its low content or poor crystallinity.

[0069] Figure 7 Comparative Example 1, scanning electron microscopy (SEM) and transmission electron microscopy (TEM) tests of WN, a is SEM image, b is TEM image, c is elemental mapping map, it can be seen that WN has a dispersed single "chain tooth" structure and each element is evenly distributed.

[0070] Figure 8Comparative Example 2 shows the scanning electron microscope (SEM) and transmission electron microscope (TEM) tests of NiFe LDH. a is the SEM image, b is the TEM image, and c is the elemental mapping diagram. It can be seen that NiFe LDH has a thin sheet-like structure with high dispersion, like a scattered "pull head" structure, and each element is evenly distributed.

[0071] Figure 9 Example 1: Scanning electron microscopy (SEM) and transmission electron microscopy (TEM) tests of WN-NiFe LDH. a is the SEM image, b is the TEM image, and c is the elemental mapping. It can be seen that WN-NiFe LDH is a heterostructure of WN connected by sheet-like NiFe LDH structures (through...). Figure 7 b, Figure 8 b, Figure 9 As can be seen from b), the two WNs are interlocked by a NiFe LDH, exhibiting a distinct zipper-like interlocking structure. Furthermore, the Ni, Fe, and O elements are more widely distributed, which is a result of the NiFe LDH acting as the "zipper head" connecting the "chain teeth" of the WNs. This interlocking structure is expected to limit catalyst distribution, thereby enabling the catalyst to possess excellent stability.

[0072] Figure 10 This indicates that the successful construction of the WN-NiFe LDH heterojunction catalyst in Example 1 significantly affected the electronic structure of both WN and NiFeLDH. These significant adjustments to the electronic structure also improved the catalytic performance and stability of the catalyst itself to some extent.

[0073] Figure 11 , 12 This study investigated the effects of different preparation conditions on the performance of the prepared catalysts (Examples 1, 2, 3, and 4), demonstrating that suitable preparation conditions (preferably a calcination temperature of 800℃ and an electrodeposition time of 600s) are crucial in determining the quality of the catalyst. (The formula for converting the measured potential to the reversible hydrogen electrode (RHE) is: E...) RHE =E Ag / AgCl +0.197 +0.059 × pH. Using 1M KOH solution as the electrolyte, linear sweep voltammetry (LSV) was performed at 10 mV / s. -1 The scan rate is recorded, and by default, all LSV curves are 90% iR corrected.

[0074] Figure 13 This demonstrates that the interaction between WN and NiFe LDH effectively improves the oxygen evolution catalytic performance relative to WN and NiFe LDH alone (Example 1, Comparative Example 1, Comparative Example 2), and exhibits superior catalytic performance compared to the OER benchmark catalyst, commercial RuO2; (linear scan conditions and...) Figure 11 same).

[0075] Figure 14 Comparative Example 1, stability test of WN (at room temperature 25°C, fixed current density 50 mA cm⁻¹) -2 (Using 1M KOH as the electrolyte, and chronovoltammetry was performed) the catalyst performed poorly, becoming deactivated after approximately 25 hours.

[0076] Figure 15 Stability tests of Example 1, Comparative Example 2, and commercial RuO2 (at room temperature 25°C, with a fixed current density of 50 mA cm⁻¹) -2 (Using 1M KOH as the electrolyte, chronovoltammetry was performed). Commercial RuO2 performed relatively poorly, deactivating after approximately 150 hours. Comparative Example 2 NiFe LDH showed better catalytic performance and stability, maintaining this for about 550 hours. Example 1 WN-NiFe LDH exhibited the best catalytic stability, with the overpotential increasing by only 35 mV after more than 4500 hours of testing, approximately 30 times that of commercial RuO2 and 7 times that of NiFe LDH.

[0077] Figure 16 Example 1: The LSV curve of WN-NiFe LDH after stability testing without iR correction shows that after more than 4500 hours of stability testing, its LSV change is negligible, demonstrating extremely strong catalytic stability.

[0078] Figure 17 After stability testing of Example 1 WN-NiFe LDH (at a fixed current density of 50 mA cm⁻¹), -2 The catalyst material was characterized and analyzed under the test conditions (4500h). The TEM images before and after the test show that the stability test has a negligible effect on the element types and distribution of the WN-NiFe LDH sample obtained in Example 1, which further confirms the stability of this catalyst material.

[0079] Figure 18 Example 1: Voltage-dependent in-situ Raman spectrum of WN-NiFe LDH. Approximately 1066 cm⁻¹. -1 The Raman peak at approximately 928 cm⁻¹ indicates the possible presence of carbonate and nitrate intercalation ions in the NiFe LDH interlayer, with peaks around 928 cm⁻¹. -1 The Raman peak at that location can be attributed to WN, 697cm -1 and 528cm -1 These correspond to Fe(OH)3 and Ni(OH)2, respectively. It is noteworthy that as the voltage increases, the Raman diffraction peaks corresponding to WN gradually disappear, and at this point, a pair of 474 cm⁻¹ peaks appear in the WN-NiFe LDH. -1 and 552cm-1 The diffraction peaks on the left and right are related to the Ni-O bending and stretching vibrations of NiOOH, which proves that NiFe LDH has undergone reconstruction and formed the active phase of Ni(Fe)OOH.

[0080] Figure 19 Voltage-dependent in-situ Raman spectra of comparative 2NiFe LDH. (Comparatively) Figure 17 A comparison clearly shows that the NiOOH characteristic peak of Example 1 WN-NiFe LDH appears at 0.35V (vs. Ag / AgCl) (overpotential of 0.14V), much earlier than that of Comparative Example 2 NiFe LDH (0.5V) (vs. Ag / AgCl) (overpotential of 0.29V). This result confirms that the presence of WN greatly accelerates the reaction of proton acceptors (such as OH-). - The transfer rate and the presence of active species effectively prevent NiFeLDH from dissolving under high voltage;

[0081] Figure 20 The CV (without iR compensation) curves of Example 1 WN-NiFe LDH and Comparative Example 2 NiFe LDH show that the redox peak of Example 1 is negatively shifted, indicating that the Ni in Example 1... 3+ The formation of active species can occur at lower sites, which further demonstrates that the introduction of WN can accelerate remodeling;

[0082] Figure 21 Based on the conclusions drawn from many current studies, under OER conditions, dissolved Fe will randomly redeposit on the surface or be doped into the host lattice. This dynamic dissolution and redeposition process leads to undesirable Fe segregation, resulting in loss of OER activity and thus decreased stability. We dynamically investigated the amount of Fe segregation in stability tests. As shown in the figure, at 50 mA / cm²... -2 In the stability test, the Fe segregation in WN-NiFe LDH was much smaller than that in NiFe LDH, and the redeposition cycle became longer and smoother. This is also an important reason for the excellent catalytic performance and stability of WN-NiFe LDH.

[0083] Figure 22 The bubble contact angles in water for Example 1 (WN-NiFe LDH) and Comparative Example 2 (NiFe LDH) are shown. The bubble contact angle of Example 1 (WN-NiFe LDH) in water is 148.10°, significantly greater than the 144.00° of NiFe LDH. This indicates that WN-NiFe LDH can release O2 more quickly and effectively avoid bubble blockage during the OER reaction, laying the foundation for its excellent activity and stability.

[0084] Figure 23Example 1, from WN-NiFe LDH at high current densities (e.g., 350 mA cm⁻¹) -2 The stability test showed that after more than 500 hours of stability testing (at room temperature of 25°C, with a fixed voltage of 1.502V vs. RHE, and 1M KOH as the electrolyte, and chronoamperometry was performed), the change in current density was negligible, demonstrating extremely strong catalytic stability, which also makes it possible to realize its application under industrial conditions.

[0085] Table 1 shows 1cm 2 The metal loading obtained by inductively coupled plasma mass spectrometry (ICP) in Example 1 and Comparative Example 2 are shown below.

[0086]

[0087]

[0088] Appendix 1 shows that, in Example 1, the metal loading of WN-NiFe LDH is approximately 1.54 mg.

[0089] Based on the above analysis, it can be seen that the interaction between the two components in the WN-NiFe LDH heterojunction not only improves the catalytic performance of the catalyst, but also allows WN-NiFe LDH to provide a 100 mA cm⁻¹ catalytic current with only a 245 mV overpotential. -2 More importantly, the interlocking effect between WN and NiFe LDH accelerates the conversion of the catalyst into an active material and effectively accelerates gas release and proton acceptor migration. Furthermore, the unique interlocking structure mutually restricts the distribution of WN and NiFe LDH. Under these effects, WN-NiFe LDH effectively reduces metal segregation, prevents bubble blockage, and avoids catalyst agglomeration, resulting in excellent OER stability and an order-of-magnitude improvement in catalytic lifetime compared to traditional commercial RuO2. This simple strategy for improving the stability and activity of NiFe-based catalysts provides a method for developing robust electrocatalysts.

Claims

1. A method for preparing WN-NiFe LDH with a zipper-tooth interlocking structure, characterized in that, Includes the following steps: Step (1): Zipper tooth-shaped WO3 is prepared using a hydrothermal method with a tungsten source. The zipper tooth-shaped WO3 is mixed with nitrogen-containing substances in a certain proportion and calcined at high temperature to obtain WN with the same zipper tooth shape. Step (1) Preparation of zipper tooth-shaped WO3: For every 1.5 mmol Na2WO4·H2O, there are 4.2 mmol H2C2O4, 1.15 mmol H8N2O8S2, and 30 mL of deionized water. After dissolution, hydrochloric acid is slowly and continuously added to adjust the pH to 1-5. After mixing evenly, purified carbon cloth (CC) is added. The reaction is carried out at 100-250 ℃ for 5-20 h. The mixture is then dried under a nitrogen atmosphere to obtain zipper tooth-shaped WO3. The obtained zipper-tooth-shaped WO3 was placed downstream of a tube furnace, with a nitrogen source placed upstream. The mixture was sintered at 600-1000 ℃ for 1-5 h to obtain zipper-tooth-shaped WN. The mass ratio of nitrogen source to WO3 was 1:2 to 50:

1. The nitrogen source was selected from melamine, dicyandiamide, and urea. Step (2): Using the zipper-shaped WN prepared in step (1) as a precursor, the final WN-NiFe LDH oxygen evolution catalyst with a zipper-shaped interlocking structure is prepared by electrochemical deposition: First, a certain proportion of Ni source and Fe source are dissolved in deionized water and mixed evenly by ultrasound and stirring to form solution A; then a certain amount of solution A is poured into the electrodeposition tank, and Ni ions and Fe ions in the solution are deposited on the zipper-shaped WN precursor by electrochemical deposition, so as to promote the formation of an interlocking structure between the zipper-shaped WN precursor and the layered NiFe metal compound, and finally obtain the highly efficient and stable oxygen evolution catalyst WN-NiFe LDH with a zipper-shaped interlocking structure.

2. The method according to claim 1, characterized in that, Step (2): Electrochemical deposition was performed using the zipper-tooth WN prepared in step (1) as the current collector; a certain proportion of Ni source and Fe source were dissolved in deionized water and mixed evenly by ultrasound and stirring to form solution A; the zipper-tooth WN was used as the working electrode, and graphite rod and Ag / AgCl were used as the counter electrode and reference electrode, respectively; electrochemical deposition was performed by chronoamperometry at a voltage of -5 V to 5 V and a deposition time of 300 s to 2000 s; the WN-NiFe LDH with zipper-tooth interlocking structure was obtained by drying under nitrogen atmosphere; The molar concentration of nickel source in solution A is 5 mM~50 mM, and the molar concentration of iron source is 5 mM~50 mM.

3. The WN-NiFe LDH with a zipper-tooth interlocking structure obtained by the method according to any one of claims 1-2, characterized in that, In the obtained catalyst, the WN surface has a tooth-like structure on one side of a zipper, and the NiFe metal layered compound NiFeLDH surface has a tooth-like structure. The teeth on the WN surface and the teeth on the NiFe LDH surface mesh to form a heterojunction with zipper-like meshing.

4. The WN-NiFe LDH with zipper tooth interlocking structure according to claim 3, characterized in that, On each side of a NiFe LDH, a WN is engaged by toothed meshing, thus forming a zipper-like interlocking structure, in which the two WNs are interlocked by a NiFe LDH.

5. The application of WN-NiFe LDH with a zipper-tooth interlocking structure as described in claim 3 or 4, as an OER catalyst.

6. The application according to claim 5, characterized in that, The stability of the obtained catalyst is maintained at a current density of 10 mA cm⁻¹ -2 ~100 mA cm -2 The time should not be less than 1000 hours.

7. The application according to claim 5, characterized in that, At 50 mA cm -2 In stability tests, Fe segregation in WN-NiFeLDH was much smaller than that in NiFe LDH; the bubble contact angle of WN-NiFe LDH in water was 148.10°; and at room temperature (25°C) and a fixed current density of 50 mA cm⁻¹, the results were satisfactory. -2 Under 1M KOH electrolyte conditions, after more than 1000 h, the overpotential increased by only 35 mV, the LSV change was negligible, and the elemental species and distribution had negligible effects; moreover, WN-NiFe LDH at >300 mA cm⁻¹ -2 It also exhibits excellent stability under high current density, and continues to release oxygen for more than 500 hours.

8. The application according to claim 5, characterized in that, In water electrolysis, WN prevents NiFe LDH from dissolving, and the introduction of WN can accelerate reconstruction.

Citation Information

Patent Citations

  • Efficient bimetallic nitride / hydroxide heterostructure electrocatalyst, preparation method and application

    CN116219484A