A method for improving crosstalk in silicon-based OLED fabrication
By directly forming chamfers in silicon-based OLED microdisplay devices using the standing wave effect, the crosstalk problem is solved, the chamfering process is saved, manufacturing efficiency is improved, costs are reduced, and product quality is improved.
Patent Information
- Application Number
- CN202311488155.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-09
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-09
AI Technical Summary
Existing silicon-based OLED microdisplay devices suffer from severe crosstalk problems, especially tandem devices, which affect the contrast and color purity of the products. Furthermore, adding an undercut process increases costs and extends the manufacturing cycle.
The chamfer is formed directly on the PDL layer by using the standing wave effect, reducing the number of chamfer fabrication steps. By utilizing the side effects of existing processes, a suitable undercut is formed by controlling the light source wavelength and exposure time, avoiding the separate exposure and etching steps for fabricating the undercut.
It optimized the product processing cycle, saved costs, improved production efficiency, reduced the negative impact of electrical crosstalk, and improved product quality.
Smart Images

Figure CN117545327B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of silicon-based OLED fabrication technology, and in particular to a method for improving crosstalk in silicon-based OLED fabrication. Background Technology
[0002] Compared to traditional AMOLED display technology, silicon-based OLED microdisplays, using single-crystal silicon chips as a substrate and leveraging mature CMOS processes, achieve smaller pixel sizes and higher integration, making them widely popular for their ability to create near-eye display products comparable to large-screen displays. Based on its technological advantages and vast market potential, silicon-based OLED microdisplays are poised to usher in a new wave of near-eye displays in both military and consumer electronics fields, bringing users an unprecedented visual experience.
[0003] Most existing silicon-based OLED full-color products use WOLED (white OLED) + CF (color filter) technology, and the device structure is generally a two-layer or single-layer Single OLED silicon-based microdisplay device. Both Single OLED and Tandem OLED silicon-based microdisplay devices face serious crosstalk problems, especially Tandem devices, which have more severe electrical crosstalk due to the presence of a CGL (color filter layer). The presence of crosstalk significantly affects the product's contrast ratio and color purity, among other optical parameters.
[0004] like Figure 8 As shown, in order to improve the crosstalk problem, an Undercut process is added to the manufacturing process to reduce pixel cascading caused by the process and interference when the light is emitted. However, adding separate exposure and etching steps for Undercut will increase the product processing cost, lengthen the production cycle, and affect the product manufacturing efficiency. Summary of the Invention
[0005] In view of the shortcomings of the existing technology, the technical problem to be solved by the present invention is to provide a method for improving crosstalk in silicon-based OLED manufacturing, so as to save the manufacturing cycle and product processing cost.
[0006] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows:
[0007] The method for improving crosstalk in silicon-based OLED fabrication includes the following steps:
[0008] S1. CMOS silicon substrate preparation;
[0009] S2. Making the anode;
[0010] S3. Create pixel layers;
[0011] S4. PDL layer exposure, the PDL layer directly forms the chamfer by enhancing the standing wave effect;
[0012] S5. PDL layer subsequent product manufacturing processes;
[0013] S6. Fabricate OLED devices.
[0014] in,
[0015] During the exposure process, an Hg lamp is used for exposure.
[0016] In step S3, the PDL pre-process is completed before PDL deposition.
[0017] The wavelength range of the light source is 240-450nm.
[0018] In step S4, a photoresist layer is formed by applying PR coating on the PDL, followed by exposure and development, and a protrusion is formed at the edge of each photoresist unit.
[0019] In step S4, during the etching process, the etching gas concentration increases around the larger the protrusion of the photoresist edge, while the concentration around the recessed edge is relatively lower. When moving to the PDL layer at a fixed rate, the concentration difference will cause a difference in the etching rate below the photoresist edge, which will cause the pattern of the photoresist layer to overlap with the PDL. The overlapped pattern is the chamfer that is needed later.
[0020] In step S4, the exposure time ranges from 3 to 6 seconds.
[0021] In step S4, the chamfer is completed and the remaining photoresist is removed.
[0022] In step S4, during the exposure process of PDL fabrication, light is reflected into the PR adhesive near the pixel area. When two waves with the same amplitude and frequency propagating in opposite directions are superimposed, a standing wave effect is formed. The PR cross-section formed by this standing wave effect matches the chamfer shape that needs to be fabricated.
[0023] The standing wave effect directly forms a chamfer. Considering the size and degree of the chamfer, the wavelength is controlled according to the combined equation of the standing wave effect, which is:
[0024] A wave propagating along the positive x-axis is called a right-traveling wave, and its wave equation is:
[0025] y1=Acos2π(t / T - x / λ ) (1)
[0026] A wave propagating along the negative x-axis is called a left-traveling wave, and its wave equation is:
[0027] y2=Acos2π(t / T + x / λ ) (2)
[0028] The combined standing wave equation is as follows:
[0029] y=y1+y2=2Acos2π(x / λ)cos2π(t / T) (3)
[0030] Where T: period; λ: wavelength; A: amplitude; t: propagation time; y: instantaneous distance between the two waves; y1: instantaneous position of the wave propagating in the positive direction; y2: instantaneous position of the wave propagating in the negative direction; x: position of the wave in the x-direction.
[0031] Compared with the prior art, the present invention has the following advantages:
[0032] This silicon-based OLED manufacturing method for improving crosstalk is reasonably designed. It reduces the original chamfering steps in the OLED process and utilizes the standing wave effect to create the chamfer. In other words, it uses the side effects of the existing process to achieve a positive effect, thereby improving product manufacturing efficiency, optimizing product processing cycle, and saving product processing costs. Attached Figure Description
[0033] The following is a brief explanation of the contents of each of the accompanying drawings and the markings in the drawings:
[0034] Figure 1 This is a diagram showing the relationship between wavelength and chamfer in this invention.
[0035] Figure 2 This is a schematic diagram of the process of the present invention.
[0036] Figure 3 This is a schematic diagram of the PDL preprocessing of the present invention.
[0037] Figure 4 This is a schematic diagram of the adhesive application process of the present invention.
[0038] Figure 5 This is a schematic diagram of the exposure and development process of the present invention.
[0039] Figure 6 This is a schematic diagram of the etching process of the present invention.
[0040] Figure 7 This is a schematic diagram illustrating the adhesive removal process of the present invention.
[0041] Figure 8 This is a schematic diagram of the existing process of the present invention. Detailed Implementation
[0042] The specific embodiments of the present invention will be further described in detail below with reference to the accompanying drawings and through the description of the examples.
[0043] like Figures 1 to 7As shown, the method for improving crosstalk in the fabrication of this silicon-based OLED includes the following steps:
[0044] S1. CMOS silicon substrate preparation;
[0045] S2. Making the anode;
[0046] S3. Create pixel layers;
[0047] S4. PDL layer exposure, the PDL layer directly forms the chamfer by enhancing the standing wave effect;
[0048] S5. PDL layer subsequent product manufacturing processes;
[0049] S6. Fabricate OLED devices.
[0050] The present invention provides a reasonable method for improving crosstalk in silicon-based OLED manufacturing. It reduces the original chamfering steps in the OLED process and utilizes the standing wave effect to create the chamfer. In other words, it uses the side effects of the existing process to achieve a positive effect, thereby improving product manufacturing efficiency, optimizing product processing cycle, and saving product processing costs.
[0051] It effectively avoids the negative impact of electrical crosstalk, improves product power consumption, and helps improve product processing efficiency. Compared with the normal process, it saves the exposure and etching steps of making the undercut separately, saving production cycle and product processing cost in the product manufacturing process. As the number of PDL layers increases, the benefits of this method in making products will become greater and greater.
[0052] During the exposure process of PDL fabrication, light is reflected into the PR resist (photoresist) near the pixel area. When two waves with the same amplitude and frequency propagating in opposite directions are superimposed, a standing wave effect is formed. The PR cross-section formed by this standing wave effect matches the shape of the required undercut. Therefore, the method proposed in this proposal is to effectively utilize this standing wave effect to directly form the undercut, reducing subsequent processing steps in the undercut fabrication process, thereby optimizing the processing flow and reducing costs. Considering the size and extent of the undercut required by the process, based on the merging equation of the standing wave effect:
[0053] A wave propagating along the positive x-axis is called a right-traveling wave, and its wave equation is:
[0054] y1=Acos2π(t / T - x / λ ) (1)
[0055] A wave propagating along the negative x-axis is called a left-traveling wave, and its wave equation is:
[0056] y2=Acos2π(t / T + x / λ ) (2)
[0057] The combined standing wave equation is as follows:
[0058] y=y1+y2=2Acos2π(x / λ)cos2π(t / T) (3)
[0059] Where T: period; λ: wavelength; A: amplitude; t: propagation time; y: instantaneous distance between the two waves; y1: instantaneous position of the wave propagating in the positive direction; y2: instantaneous position of the wave propagating in the negative direction; x: position of the wave in the x-direction.
[0060] like Figure 1 As shown, the relationship between wavelength and undercut shape is that shortening the wavelength λ of the incident light source (by changing to a different exposure light source) can increase the density of the undercut protrusions in the PDL layer, so as to create a suitable undercut and achieve a proper reduction of the influence of crosstalk.
[0061] In addition, such as Figure 2 The new undercut fabrication method is based on the fact that the materials used in the undercut and PDL fabrication are the same. During the PDL fabrication process, the wavelength of the light source used in the exposure process is controlled (i.e., different types of light sources, generally Hg lamps, and the corresponding tables of commonly used light sources and wavelengths are shown in the table below) to achieve the undercut fabrication.
[0062] Table 1: Light Source and Wavelength Correspondence Table
[0063]
[0064] Preferably, during the exposure process, a light source is used for exposure, and the light source is an Hg lamp; the wavelength range of the light source is 240-450nm.
[0065] This invention mainly improves the PDL manufacturing process; other manufacturing processes can be completed using existing methods. A preferred specific example of the PDL manufacturing process is as follows:
[0066] After completing the pre-PDL process, PDL deposition is then performed.
[0067] Photoresist is applied to the PDL to form a photoresist layer, followed by exposure and development, resulting in protrusions at the edges of each photoresist unit.
[0068] According to the standing wave effect equation, the greater the requirement for undercut prominence, the shorter the wavelength of the light source should be. The selection of the light source and the exposure duration should be based on actual needs. Generally, the exposure duration of a single field (field of view) is increased by 0.1-3 seconds; the exposure time range is 3-6 seconds.
[0069] During the etching process, when the etching gas approaches the raised edge, the concentration of etching gas near the larger raised edge of the photoresist increases, while the concentration near the recessed edge increases relatively less. When moving to the PDL layer at a fixed rate, the concentration difference will cause the etching rate below the photoresist edge to differ, which will cause the pattern of the photoresist layer to overlap with the PDL. The overlapped pattern is the chamfer that is needed later.
[0070] Complete the chamfering and shaping, and remove the remaining photoresist.
[0071] Compared with the normal process, the present invention saves the exposure and etching steps of making the undercut separately, saves the production cycle and product processing costs in the product manufacturing process, and improves product processing efficiency.
[0072] The present invention has been described above by way of example with reference to the accompanying drawings. Obviously, the specific implementation of the present invention is not limited to the above-described manner. Any non-substantial improvements made using the concept and technical solution of the present invention, or the direct application of the concept and technical solution of the present invention to other occasions without modification, are all within the protection scope of the present invention.
Claims
1. A method for improving crosstalk in silicon-based OLED fabrication, characterized in that: Includes the following steps: S1. CMOS silicon substrate preparation; S2. Making the anode; S3. Create pixel layers; S4. PDL layer exposure: The PDL layer directly forms the chamfer by enhancing the standing wave effect; S5. Subsequent product manufacturing processes for the PDL layer; S6. Fabrication of OLED devices; in, In step S4, a photoresist layer is formed by coating the PDL with PR, followed by exposure and development. During the exposure process, light is reflected into the PR resin near the pixel area. When two waves with the same amplitude and frequency propagating in opposite directions are superimposed, a standing wave effect is formed. This standing wave effect forms a PR cross section with a protrusion, which causes the pattern of the photoresist layer to be overlaid on the PDL to form a chamfer. The remaining photoresist is then removed.
2. The method for improving crosstalk in silicon-based OLED fabrication as described in claim 1, characterized in that: During the exposure process, an Hg lamp is used for exposure.
3. The method for improving crosstalk in silicon-based OLED fabrication as described in claim 1, characterized in that: In step S3, the PDL pre-process is completed before PDL deposition.
4. The method for improving crosstalk in silicon-based OLED fabrication as described in claim 2, characterized in that: The wavelength range of the light source is 240-450nm.
5. The method for improving crosstalk in silicon-based OLED fabrication as described in claim 1, characterized in that: In step S4, the exposure time ranges from 3 to 6 seconds.
6. The method for improving crosstalk in silicon-based OLED fabrication as described in claim 1, characterized in that: The standing wave effect directly forms a chamfer. Considering the size and degree of the chamfer, the wavelength is controlled according to the combined equation of the standing wave effect, which is: A wave propagating along the positive x-axis is called a right-traveling wave, and its wave equation is: y1=Acos2π(t / T - x / λ) (1) A wave propagating along the negative x-axis is called a left-traveling wave, and its wave equation is: y2=Acos2π(t / T + x / λ) (2) The combined standing wave equation is as follows: y=y1+y2=2Acos2π(x / λ)cos2π(t / T) (3) Where T: period; λ: wavelength; A: amplitude; t: propagation time; y: instantaneous distance between the two waves; y1: instantaneous position of the wave propagating in the positive direction; y2: instantaneous position of the wave propagating in the negative direction; x: position of the wave in the x-direction.
Citation Information
Patent Citations
Photoresist back exposure process
CN102566313A
Pattern laminating substrate available multi-transferring and method of laminating the pattern by using the same