Elastic nonwoven fabric and its production process and application
By using TPU and antioxidants in the production process of elastic nonwovens, combined with optimizing process parameters, the problem of easy damage and insufficient performance of ordinary elastic nonwovens is solved, and nonwovens with high strength, good elasticity and durability are prepared. Woven fabrics for a variety of applications.
Patent Information
- Application Number
- CN202311505777.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2023-10-31
- Filing Date
- 2023-11-13
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-11-13
AI Technical Summary
Ordinary elastic nonwovens are easily damaged by daily use and environmental factors, and have low air permeability, softness and poor wear resistance, which limits their application areas.
A nonwoven manufacturing process including TPU and antioxidants is used to form a fiber network structure with high strength and good elasticity through mixing and drying, melt extrusion, filtration, metering, spinning and cooling steps. Combining optimized process parameters such as temperature, pressure and hot air treatment, nonwoven fabrics with good elasticity, softness, abrasion resistance, waterproofness and breathability are prepared.
Achieving high strength, good elasticity, comfort and durability of elastic nonwovens, suitable for a variety of applications, such as shoe materials, clothing linings and medical dressings, extending the service life and improving the chemical resistance of the material performance.
Smart Images

Figure BDA0004545800830000131 
Figure BDA0004545800830000141
Abstract
Description
Technical Field
[0001] The present application relates to an elastic nonwoven fabric, a manufacturing process and application thereof, and belongs to the field of nonwoven fabric manufacturing. Background Art
[0002] Elastic nonwoven fabric is a kind of fabric made of fiber or fiber combination through nonwoven process. Compared with traditional woven fabric, elastic nonwoven fabric does not need to go through the process of weaving and knitting, but combines the fibers together by melting, bonding or mechanical processing.
[0003] Ordinary elastic nonwoven fabrics are easily damaged and deteriorated by daily use and environmental factors, are easily penetrated and wetted by water, and have low air permeability and poor softness and elasticity, which limit the application areas of elastic nonwoven fabrics. Summary of the invention
[0004] In order to solve the above problems, an elastic nonwoven fabric and its production process and application are provided, so that the elastic nonwoven fabric has the advantages of good elasticity, softness, wear resistance, waterproofness, air permeability, oxidation resistance and weather resistance, and can be suitable for various application fields.
[0005] The present invention provides the following technical solutions:
[0006] An elastic nonwoven fabric comprises the following components in parts by weight:
[0007] TPU 90-110 parts, antioxidant 0.1-3 parts.
[0008] Preferably, the soft segment structure in the TPU is at least one of PBA, PTMEG, PCL, and bio-based polyol.
[0009] Preferably, the soft segment structure in the TPU is PBA or PTMEG.
[0010] Preferably, the hard segment structure in the TPU is at least one of MDI, HDI, IPDI and NDI.
[0011] Preferably, the hard segment structure in the TPU is MDI or IPDI.
[0012] Preferably, the Shore hardness of the TPU is 65A-75D.
[0013] Preferably, the antioxidant is a mixture of one or more of an ester antioxidant, an amine antioxidant or a phenolic antioxidant.
[0014] According to one aspect of the present application, there is provided a process for producing an elastic nonwoven fabric as described above, comprising the following steps:
[0015] (1) Mixing and drying: Mixing TPU and antioxidant and drying them, and adding them into a mixer for mixing to obtain polymer chips;
[0016] (2) Melt extrusion: Place the polymer slices into a screw extruder, adjust the speed and box temperature of the screw extruder, and the polymer slices are heated and melted in the screw extruder to form a viscous melt, which is compressed by the extruder and transported to the melt pipe;
[0017] (3) Filtration: The melt is transported to the filter, where impurities and unmelted particles are filtered out through the filter;
[0018] (4) Metering: The filtered melt flows through a metering pump, the pressure of which is adjusted to accurately meter the polymer and deliver it continuously and stably into the spinning machine;
[0019] (5) Spinning into a web: After the melt enters the die and is mixed evenly, it is evenly distributed in each spinning hole of the spinneret, and a fine stream is evenly ejected from the spinning hole. Finally, short fibers are formed after being pulled by hot air, and the short fibers form a web on the mesh curtain;
[0020] (6) Cooling: After the web is formed, it is further cooled by a cold air system to obtain a fabric sample;
[0021] (7) Stretching and winding: Winding the cooled fabric sample.
[0022] Preferably, in step (1), the drying temperature is 80-120° C., and the drying time is 2-4 hours.
[0023] Preferably, in step (2), the screw speed is 100-300 r / min, the screw temperature in the first zone is 80°C-150°C, in the second zone is 150°C-200°C, in the third zone is 170°C-230°C, in the fourth zone: 170°C-250°C, and in the fifth zone is 170°C-260°C.
[0024] Preferably, in step (4), the pressure of the metering pump is 5-40 MPa;
[0025] Preferably, in step (5), the temperature of the extrusion die in the first zone is 200°C-260°C, the second zone is 200°C-260°C, the third zone is 200°C-260°C, and the fourth zone is 200°C-260°C; the hot air pressure is 5-30MPa, and the hot air temperature is 210°C-270°C; the distance between the die and the mesh curtain is 10-50cm.
[0026] In the step (6), the winding speed is 5-30 m / min.
[0027] According to another aspect of the present application, there is also provided an application in shoe materials, clothing linings, medical dressings, menstrual pants, sanitary pants, and facial mask base fabrics.
[0028] In the present application, "PBA" means polyester polyol, "PTMEG" means polyether polyol, "PCL" means polycarbonate polyol, "MDI" means diphenylmethane diisocyanate, "HDI" means hexamethylene diisocyanate, "IPDI" means isophorone diisocyanate, and "NDI" means naphthalene diisocyanate.
[0029] The beneficial effects of this application include but are not limited to:
[0030] 1. The elastic nonwoven fabric provided in the present application has appropriate softness, hardness, tensile strength and antioxidant properties to meet the needs of different application scenarios and improve its service life.
[0031] 2. The elastic nonwoven fabric provided in the present application is added with thermoplastic polyurethane, so that the nonwoven fabric has good elasticity and can adapt to surfaces of different shapes and curves, providing better comfort and fit for the obtained nonwoven fabric.
[0032] 3. The manufacturing process of an elastic nonwoven fabric provided in the present application adopts a melt-blown process. The melt-blown process can make TPU and antioxidants evenly mixed, and melted into fibers at high temperature to form a high-strength fiber mesh structure. This makes the elastic nonwoven fabric have better strength and wear resistance, and can withstand greater stretching and tearing forces; TPU itself has excellent elasticity and resilience, and the elastic nonwoven fabric prepared by the melt-blown process can maintain its original elastic properties. This makes the fabric have better adaptability and comfort, and can provide better support and protection; the melt-blown process can control the porosity and distribution of the fibers, so that the elastic nonwoven fabric has better air permeability and moisture regulation; TPU itself has good chemical resistance, and with the addition of antioxidants, the elastic nonwoven fabric has better chemical resistance.
[0033] 4. The present application provides a manufacturing process for an elastic nonwoven fabric, with optimized production process parameters. After the TPU and antioxidant are mixed and dried through the mixing, drying and melt extrusion steps, a viscous melt is formed through the heating and extrusion of a screw extruder. This preparation method can make the melt uniform and stable, which is beneficial to the quality control of subsequent spinning and web forming. By optimizing the drying temperature and duration, the raw materials can be fully mixed and dried, and the uniformity and stability of the subsequent melt can be improved; through the filtering step, the melt is filtered through the filter screen, which can effectively remove impurities and unmelted particles, and ensure the fiber quality during the spinning and web forming process. By optimizing the design of the filter and selecting an appropriate filter screen, the filtering effect can be improved and the fiber quality can be further improved; by adjusting the metering pump, the continuous and stable delivery of the filtered melt can be achieved, ensuring the fiber uniformity and stability during the spinning and web forming process. By optimizing the pressure of the metering pump, the flow rate of the melt can be controlled, and the uniformity and stability of the fiber can be further improved; after the melt enters the die head, a fine stream is uniformly ejected through the spinneret hole, and short fibers are formed after being pulled by the hot air flow, and finally formed into a web on the mesh curtain. By controlling the extrusion die temperature, hot air temperature, and the distance between the die and the mesh curtain, the uniformity and stability of the spinning web can be achieved. By optimizing the extrusion die temperature and hot air parameters, the thickness and tension of the fiber can be controlled, and the uniformity and stability of the fiber can be further improved; by cooling through the cold air system, the fiber can be further solidified to obtain a fabric sample. The cooled fabric sample is then stretched and rolled for subsequent processing and use. By controlling the cooling speed and rolling speed, the performance and appearance of the fabric sample can be adjusted. DETAILED DESCRIPTION
[0034] The present invention is further described below in conjunction with specific embodiments. It is pointed out that the following embodiments cannot be understood as limiting the scope of protection of the present invention. Simple substitutions or adjustments made by ordinary technicians in the field based on the contents of the present invention are all within the scope of protection of the present invention.
[0035] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0036] Example 1
[0037] The specific parameters of the manufacturing process of the above elastic nonwoven fabric are as follows:
[0038] (1) Mixing and drying: 90 parts of TPU and 0.1 parts of ester antioxidant are mixed and dried at a temperature of 80° C. for 2 hours, and then added into a mixer for mixing to obtain polymer chips, wherein the soft segment structure of TPU is PBA, and the hard segment structure of TPU is MDI; the Shore hardness of TPU is 65A;
[0039] (2) Melt extrusion: Place the polymer slices in a screw extruder, adjust the speed of the screw extruder to 100 r / min, the first zone of the screw extruder to 80°C, the second zone to 150°C, the third zone to 170°C, the fourth zone to 170°C, and the fifth zone to 170°C. The polymer slices are heated and melted in the screw extruder to form a viscous melt, which is compressed by the extruder and transported to the melt pipe;
[0040] (3) Filtration: The melt is extruded and transported to the filter, where impurities and unmelted particles are filtered out through the filter;
[0041] (4) Metering: The filtered melt flows through a metering pump, and the pressure of the metering pump is adjusted to 5 MPa to continuously and stably transport the filtered melt into the spinning machine;
[0042] (5) Spinning into a web: The die temperature is set to 200°C for the first zone, 200°C for the second zone, 200°C for the third zone, and 200°C for the fourth zone. After the melt enters the die and is mixed evenly, a thin stream is uniformly ejected from the spinneret hole. Finally, short fibers are formed by hot air traction at a pressure of 5 MPa and a temperature of 210°C. The short fibers are webbed on a mesh curtain. The distance between the die and the mesh curtain is 10 cm.
[0043] (6) Cooling: After the web is formed, it is further cooled by a cold air system to obtain a fabric sample;
[0044] (7) Stretching and winding: Wind the cooled fabric sample at a winding speed of 5 m / min.
[0045] Example 2
[0046] The specific parameters of the manufacturing process of the above elastic nonwoven fabric are as follows:
[0047] (1) Mixing and drying: 100 parts of TPU and 1.2 parts of phenolic antioxidant are mixed and dried at a temperature of 120° C. for 4 hours, and then added into a mixer for mixing to obtain polymer chips, wherein the soft segment structure of TPU is PTMEG, and the hard segment structure of TPU is HDI; the Shore hardness of TPU is 75A;
[0048] (2) Melt extrusion: Place the polymer slices in a screw extruder, adjust the speed of the screw extruder to 300 r / min, the first zone of the screw extruder to 150°C, the second zone to 200°C, the third zone to 230°C, the fourth zone to 250°C, and the fifth zone to 260°C. The polymer slices are heated and melted in the screw extruder to form a viscous melt, which is compressed by the extruder and transported to the melt pipe;
[0049] (3) Filtration: The melt is extruded and transported to the filter, where impurities and unmelted particles are filtered out through the filter;
[0050] (4) Metering: The filtered melt flows through a metering pump, and the pressure of the metering pump is adjusted to 40 MPa to continuously and stably transport the filtered melt into the spinning machine;
[0051] (5) Spinning into a web: The die temperature is set to 200°C-260°C for the first zone, 200°C-260°C for the second zone, 200°C-260°C for the third zone, and 200°C-260°C for the fourth zone. After the melt enters the die and is mixed evenly, it is evenly distributed in each spinning hole of the spinneret, and fine streams are evenly ejected from the spinning holes. Finally, short fibers are formed by hot air traction with a wind pressure of 5-30 MPa and a temperature of 210°C-270°C. The short fibers are webbed on a mesh curtain, and the distance between the die and the mesh curtain is 10-50 cm.
[0052] (6) Cooling: After the web is formed, it is further cooled by a cold air system to obtain a fabric sample;
[0053] (7) Stretching and winding: Wind the cooled fabric sample at a speed of 5-30 m / min.
[0054] Example 3
[0055] The specific parameters of the manufacturing process of the above elastic nonwoven fabric are as follows:
[0056] (1) Mixing and drying: 98 parts of TPU and 0.8 parts of amine antioxidant are mixed and dried at a temperature of 100° C. for 3 hours, and then added into a mixer for mixing to obtain polymer chips, wherein the soft segment structure of TPU is PCL, and the hard segment structure of TPU is IPDI; the Shore hardness of TPU is 80A;
[0057] (2) Melt extrusion: Place the polymer slices in a screw extruder, adjust the speed of the screw extruder to 150 r / min, the first zone of the screw extruder to 100°C, the second zone to 180°C, the third zone to 230°C, the fourth zone to 250°C, and the fifth zone to 230°C. The polymer slices are heated and melted in the screw extruder to form a viscous melt, which is compressed by the extruder and transported to the melt pipe;
[0058] (3) Filtration: The melt is extruded and transported to the filter, where impurities and unmelted particles are filtered out through the filter;
[0059] (4) Metering: The filtered melt flows through a metering pump, and the pressure of the metering pump is adjusted to 30 MPa to continuously and stably transport the filtered melt into the spinning machine;
[0060] (5) Spinning into a web: The die temperature is set to 210°C for the first zone, 220°C for the second zone, 220°C for the third zone, and 230°C for the fourth zone. After the melt enters the die and is mixed evenly, it is evenly distributed in each spinning hole of the spinneret, and a thin stream is evenly ejected from the spinning hole. Finally, short fibers are formed by hot air traction at a pressure of 15 MPa and a temperature of 240°C. The short fibers are webbed on a mesh curtain, and the distance between the die and the mesh curtain is 30 cm.
[0061] (6) Cooling: After the web is formed, it is further cooled by a cold air system to obtain a fabric sample;
[0062] (7) Stretching and winding: Wind the cooled fabric sample at a speed of 25 m / min.
[0063] Example 4
[0064] The specific parameters of the manufacturing process of the above elastic nonwoven fabric are as follows:
[0065] (1) Mixing and drying: 95 parts of TPU and 2 parts of a mixture of an ester antioxidant and an amine antioxidant are mixed and dried at a temperature of 100° C. for 3 hours, and then added into a mixer for mixing to obtain polymer chips, wherein the soft segment structure of TPU is PBA, and the hard segment structure of TPU is MDI; the Shore hardness of TPU is 65D;
[0066] (2) Melt extrusion: Place the polymer slices in a screw extruder, adjust the speed of the screw extruder to 250 r / min, the first zone of the screw extruder to 100°C, the second zone to 180°C, the third zone to 200°C, the fourth zone to 210°C, and the fifth zone to 220°C. The polymer slices are heated and melted in the screw extruder to form a viscous melt, which is compressed by the extruder and transported to the melt pipe;
[0067] (3) Filtration: The melt is extruded and transported to the filter, where impurities and unmelted particles are filtered out through the filter;
[0068] (4) Metering: The filtered melt flows through a metering pump, and the pressure of the metering pump is adjusted to 32 MPa to continuously and stably transport the filtered melt into the spinning machine;
[0069] (5) Spinning into a web: The die temperature is set to 220°C for the first zone, 230°C for the second zone, 240°C for the third zone, and 250°C for the fourth zone. After the melt enters the die and is mixed evenly, it is evenly distributed in each spinning hole of the spinneret, and a thin stream is evenly ejected from the spinning hole. Finally, short fibers are formed by hot air traction with a wind pressure of 18 MPa and a temperature of 250°C. The short fibers are webbed on a mesh curtain, and the distance between the die and the mesh curtain is 30 cm.
[0070] (6) Cooling: After the web is formed, it is further cooled by a cold air system to obtain a fabric sample;
[0071] (7) Stretching and winding: Wind the cooled fabric sample at a speed of 18 m / min.
[0072] Example 5
[0073] The specific parameters of the manufacturing process of the above elastic nonwoven fabric are as follows:
[0074] (1) Mixing and drying: 100 parts of TPU and 1.2 parts of a mixture of an ester antioxidant and a phenolic antioxidant are mixed and dried at a temperature of 90° C. for 3 hours, and added into a mixer for mixing to obtain polymer chips, wherein the soft segment structure of the TPU is a bio-based polyol, and the hard segment structure of the TPU is NDI; the Shore hardness of the TPU is 70D;
[0075] (2) Melt extrusion: Place the polymer slices in a screw extruder, adjust the speed of the screw extruder to 170 r / min, the first zone of the screw extruder to 110°C, the second zone to 150°C, the third zone to 200°C, the fourth zone to 210°C, and the fifth zone to 240°C. The polymer slices are heated and melted in the screw extruder to form a viscous melt, which is compressed by the extruder and transported to the melt pipe;
[0076] (3) Filtration: The melt is extruded and transported to the filter, where impurities and unmelted particles are filtered out through the filter;
[0077] (4) Metering: The filtered melt flows through the metering pump, and the pressure of the metering pump is adjusted to 20 MPa to continuously and stably transport the filtered melt into the spinning machine;
[0078] (5) Spinning into a web: The die temperature is set to 210°C for the first zone, 220°C for the second zone, 240°C for the third zone, and 250°C for the fourth zone. After the melt enters the die and is mixed evenly, it is evenly distributed in each spinning hole of the spinneret, and a thin stream is evenly ejected from the spinning hole. Finally, short fibers are formed by hot air traction at a pressure of 24 MPa and a temperature of 270°C. The short fibers are webbed on a mesh curtain. The distance between the die and the mesh curtain is 40 cm.
[0079] (6) Cooling: After the web is formed, it is further cooled by a cold air system to obtain a fabric sample;
[0080] (7) Stretching and winding: Wind the cooled fabric sample at a speed of 26 m / min.
[0081] Example 6
[0082] The specific parameters of the manufacturing process of the above elastic nonwoven fabric are as follows:
[0083] (1) Mixing and drying: 95 parts of TPU, 2.5 parts of a mixture of an ester antioxidant, an amine antioxidant and a phenolic antioxidant are mixed and dried at a temperature of 120° C. for 4 hours, and added into a mixer for mixing to obtain polymer chips, wherein the soft segment structure of the TPU is PBA, and the hard segment structure of the TPU is IPDI; the Shore hardness of the TPU is 65D;
[0084] (2) Melt extrusion: Place the polymer slices in a screw extruder, adjust the speed of the screw extruder to 200 r / min, the first zone of the screw extruder to 110°C, the second zone to 180°C, the third zone to 200°C, the fourth zone to 210°C, and the fifth zone to 220°C. The polymer slices are heated and melted in the screw extruder to form a viscous melt, which is compressed by the extruder and transported to the melt pipe;
[0085] (3) Filtration: The melt is extruded and transported to the filter, where impurities and unmelted particles are filtered out through the filter;
[0086] (4) Metering: The filtered melt flows through a metering pump, and the pressure of the metering pump is adjusted to 10 MPa to continuously and stably transport the filtered melt into the spinning machine;
[0087] (5) Spinning into a web: The die temperature is set to 220°C in the first zone, 240°C in the second zone, 240°C in the third zone, and 250°C in the fourth zone. After the melt enters the die and is evenly mixed, it is evenly distributed in each spinning hole of the spinneret, and a thin stream is evenly ejected from the spinning hole. Finally, short fibers are formed by hot air traction with a wind pressure of 29 MPa and a temperature of 220°C. The short fibers are webbed on a mesh curtain, and the distance between the die and the mesh curtain is 10-50 cm;
[0088] (6) Cooling: After the web is formed, it is further cooled by a cold air system to obtain a fabric sample;
[0089] (7) Stretching and winding: Wind the cooled fabric sample at a speed of 15 m / min.
[0090] Example 7
[0091] (1) Mixing and drying: 95 parts of TPU, 2.5 parts of a mixture of an ester antioxidant, an amine antioxidant and a phenolic antioxidant are mixed and dried at a temperature of 120° C. for 4 hours, and added into a mixer for mixing to obtain polymer chips, wherein the soft segment structure of the TPU is PTMEG, and the hard segment structure of the TPU is HDI; the Shore hardness of the TPU is 60A;
[0092] (2) Melt extrusion: Place the polymer slices in a screw extruder, adjust the speed of the screw extruder to 200 r / min, the first zone of the screw extruder to 110°C, the second zone to 180°C, the third zone to 200°C, the fourth zone to 210°C, and the fifth zone to 220°C. The polymer slices are heated and melted in the screw extruder to form a viscous melt, which is compressed by the extruder and transported to the melt pipe;
[0093] (3) Filtration: The melt is extruded and transported to the filter, where impurities and unmelted particles are filtered out through the filter;
[0094] (4) Metering: The filtered melt flows through the metering pump, and the pressure of the metering pump is adjusted to 15 MPa to continuously and stably transport the filtered melt into the spinning machine;
[0095] (5) Spinning into a web: The die temperature is set to 220°C in the first zone, 240°C in the second zone, 240°C in the third zone, and 250°C in the fourth zone. After the melt enters the die and is evenly mixed, it is evenly distributed in each spinning hole of the spinneret, and a thin stream is evenly ejected from the spinning hole. Finally, short fibers are formed by hot air traction with a wind pressure of 29 MPa and a temperature of 220°C. The short fibers are webbed on a mesh curtain, and the distance between the die and the mesh curtain is 10-50 cm;
[0096] (6) Cooling: After forming the web, it is further cooled by a cold air system to obtain a fabric sample; (7) Stretching and winding: The cooled fabric sample is wound up at a winding speed of 15 m / min.
[0097] Example 8
[0098] The specific parameters of the manufacturing process of the above elastic nonwoven fabric are as follows:
[0099] (1) Mixing and drying: 100 parts of TPU and 1.2 parts of a mixture of an ester antioxidant and a phenolic antioxidant are mixed and dried at a temperature of 90° C. for 3 hours, and then added into a mixer for mixing to obtain polymer chips. Specifically, the soft segment structure of the TPU is PBA, and the hard segment structure of the TPU is HDI; the Shore hardness of the TPU is 80A;
[0100] (2) Melt extrusion: Place the polymer slices in a screw extruder, adjust the speed of the screw extruder to 170 r / min, the first zone of the screw extruder to 110°C, the second zone to 150°C, the third zone to 200°C, the fourth zone to 210°C, and the fifth zone to 240°C. The polymer slices are heated and melted in the screw extruder to form a viscous melt, which is compressed by the extruder and transported to the melt pipe;
[0101] (3) Filtration: The melt is extruded and transported to the filter, where impurities and unmelted particles are filtered out through the filter;
[0102] (4) Metering: The filtered melt flows through the metering pump, and the pressure of the metering pump is adjusted to 32 MPa to continuously and stably transport the filtered melt into the spinning machine;
[0103] (5) Spinning into a web: The die temperature is set to 210°C for the first zone, 220°C for the second zone, 240°C for the third zone, and 250°C for the fourth zone. After the melt enters the die and is mixed evenly, it is evenly distributed in each spinning hole of the spinneret, and a thin stream is evenly ejected from the spinning hole. Finally, short fibers are formed by hot air traction at a pressure of 24 MPa and a temperature of 270°C. The short fibers are webbed on a mesh curtain. The distance between the die and the mesh curtain is 40 cm.
[0104] (6) Cooling: After forming the web, the web is further cooled by a cold air system to obtain a fabric sample; (7) Stretching and winding: The cooled fabric sample is wound at a speed of 26 m / min.
[0105] Comparative Example 1
[0106] Compared with Example 4, Comparative Example 1 differs in that, in the specific parameters of the production process of the elastic nonwoven fabric, in step (1), the number of parts of TPU is increased to 120 parts.
[0107] Comparative Example 2
[0108] Compared with Example 4, Comparative Example 2 differs in that, in the specific parameters of the manufacturing process of the elastic nonwoven fabric, in step (1), TPU is replaced by PP.
[0109] Comparative Example 3
[0110] Compared with Example 4, Comparative Example 3 differs in that, in the specific parameters of the manufacturing process of the elastic nonwoven fabric, no antioxidant is added in step (1).
[0111] Comparative Example 4
[0112] Compared with Example 4, the difference between Comparative Example 4 and Example 4 is that, in the specific parameters of the production process of the elastic non-woven fabric, in step (2), the temperatures of each zone of the screw are set to 150°C in the first zone, 210°C in the second zone, 240°C in the third zone, 270°C in the fourth zone, and 300°C in the fifth zone.
[0113] Comparative Example 5
[0114] Comparative Example 5 is different from Example 4 in that the specific parameters of the production process of the elastic nonwoven fabric are as follows: in step (4), the pressure of the metering pump is adjusted to 70 MPa.
[0115] Comparative Example 6
[0116] Compared with Example 4, Comparative Example 6 differs in that, in the specific parameters of the production process of the elastic nonwoven fabric, in step (5), the hot air temperature is set to 100°C.
[0117] Comparative Example 7
[0118] Compared with Example 4, Comparative Example 7 differs in that, in the specific parameters of the production process of the nonwoven fabric, in step (5), the distance between the die head and the mesh curtain is 5 cm.
[0119] The tensile strength, elongation at break, hardness, wear resistance and air permeability of the wear-resistant and low-noise materials prepared in the above comparative examples and embodiments were tested; the test results are shown in Table 1.
[0120] Table 1
[0121]
[0122]
[0123] As can be seen from the above table, the raw material ratio and production process used in this application can obtain an elastic nonwoven fabric with good tensile strength, high wear resistance and good air permeability; it can adapt to surfaces of different shapes and curves, provide better comfort and fit for the obtained nonwoven fabric, and expand its application environment. When the hardness of TPU increases, it means that the material becomes more rigid and hard. This will cause the softness and bending performance of the elastic cloth to decrease, causing it to lose some of its elasticity. The elastic recovery ability and tensile properties of the elastic cloth are affected, making it unable to meet specific application requirements. Elastic cloth is generally used in applications that require comfort and fit, such as clothing linings, footwear and bedding. When the hardness of TPU exceeds a certain range, the comfort of the elastic cloth may decrease. Increased hardness will increase the rigidity of the material, making it feel harder when it contacts the skin, which may reduce the comfort of the user; reduced hardness of TPU means that the material is softer, which may lead to insufficient elasticity of the elastic nonwoven fabric. The material may be too soft and unable to provide sufficient resilience and support, thereby affecting its elastic properties. Low hardness TPU materials generally have lower wear resistance. During the use of elastic nonwovens, if the hardness of the material is too low, the surface of the material may be easily worn and damaged, reducing its durability and service life. TPU materials with low hardness may be more sensitive to chemicals and easily corroded and damaged. This may limit the use of elastic nonwovens in specific environments, especially in applications that come into contact with chemicals. TPU materials with low hardness may be difficult to handle during processing. Excessively soft materials may make it difficult to control viscosity and shape during processing, and special processing methods and processes may be required; it can also be seen from the above table that in Example 4, the elastic nonwoven obtained has the best performance.
[0124] Comparative Example 1 is different from Example 4 in that, in the specific parameters of the manufacturing process of the elastic nonwoven fabric, in step (1), the number of TPU parts is increased to 120 parts. Decreased elastic properties: Too much TPU may make the elastic nonwoven fabric too hard, lose some of its softness and bending properties, reduce the elastic recovery ability and tensile properties of the material, and make it unable to meet specific application requirements. Moreover, too much TPU may make the material more sticky and viscous, increasing the difficulty of handling during processing. Higher temperatures and greater pressures may be required to ensure the melting and formation of the material, increasing the complexity and cost of the preparation process.
[0125] Compared with Example 4, Comparative Example 2 differs in that, in the specific parameters of the manufacturing process of the elastic nonwoven fabric, in step (1), TPU is replaced by PP.
[0126] Compared with TPU, PP has lower strength and wear resistance. Therefore, replacing TPU with PP may weaken the elasticity and softness of the product, causing it to lose some of its elasticity and resilience. In addition, TPU has good chemical resistance and can withstand the erosion of some chemicals. While PP may swell or dissolve in certain chemicals, TPU usually has good thermal stability and can maintain good performance in high temperature environments. However, PP has poor thermal stability and is prone to softening and deformation, which limits its application areas.
[0127] The difference between Comparative Example 3 and Example 4 is that without adding an antioxidant, the strength and hardness of the elastic nonwoven fabric are affected, and the weather resistance is reduced, resulting in a shortened service life of the product outdoors or in harsh environments, affecting the application range and performance of the material.
[0128] Compared with Example 4, Comparative Example 4 is different in that the specific parameters of the manufacturing process of the elastic nonwoven fabric are as follows: in step (2), the temperatures of the screw zones are set to 150°C in the first zone, 210°C in the second zone, 240°C in the third zone, 270°C in the fourth zone, and 300°C in the fifth zone. This causes the viscous dissipation of the deformation energy stored in the melt during the flow to increase, resulting in a weakening of the elastic characteristics. After the melt stream is extruded through the spinneret hole, the fiber fineness is reduced, the diameter is reduced, the porosity is reduced, and the air permeability of the material is deteriorated. In particular, when the material is applied to the fields of clothing lining, medical dressings, menstrual pants, sanitary pants, and facial mask base fabrics, the material is required to have high air permeability and softness. The above-mentioned setting changes cannot meet the requirements of the application field.
[0129] Comparative Example 5 is different from Example 4 in that, in the specific parameters of the manufacturing process of the elastic nonwoven fabric, in step (4), the metering pump pressure is adjusted to 70 MPa. Excessive metering pump pressure will increase the flow rate of the melt, making the fiber stretching during the spinning process uneven. This may lead to inconsistent fiber thickness and uneven fiber distribution, thereby reducing the quality of the elastic nonwoven fabric. Excessive metering pump pressure will also increase the tension of the fibers during the spinning process, exceeding the bearing capacity of the fibers, resulting in fiber breakage. This will lead to uneven fiber length and the presence of broken fibers, reducing the strength and durability of the elastic nonwoven fabric, and cannot meet the requirements for high softness of the material when the material is used in the fields of clothing linings, medical dressings, menstrual pants, sanitary pants, and facial mask base fabrics.
[0130] Compared with Example 4, Comparative Example 6 is different in that in step (5), the hot air temperature is set to 100° C. The hot air temperature can affect the melt temperature through heat conduction of the spinneret on the meltblowing die head, but when the temperature is too high, the nonwoven fabric will become hard and brittle, and cannot meet the requirements of high softness of the material when the material is used in the fields of clothing lining, medical dressings, menstrual pants, sanitary pants, facial mask base fabrics, etc.
[0131] Compared with Example 4, Comparative Example 7 is different in that, in step (5), the distance between the die head and the mesh curtain is 5 cm. The distance between the die head and the mesh curtain determines the crystallization speed and porosity of the nonwoven fabric, further affecting its tear strength and transverse and longitudinal tension; the distance between the die head and the mesh curtain will also affect the degree of stretching of the fiber. A larger distance will cause the fiber to stretch longer during the ejection process, thereby obtaining longer fibers. A relatively smaller distance will reduce the degree of fiber stretching, resulting in shorter fibers. Moreover, the distance between the die head and the mesh curtain will also affect the orientation of the fiber after ejection. A larger distance will make the fiber more susceptible to external wind force after ejection, thereby making the orientation of the fiber more parallel. On the contrary, a smaller distance will cause the fiber to be subject to greater resistance, and the orientation of the fiber may be more random. The orientation of the fiber affects the strength, air permeability and feel of the nonwoven fabric, and cannot meet the application requirements.
[0132] The above is only the embodiment of the present application, and the protection scope of the present application is not limited by these specific embodiments, but is determined by the claims of the present application. For those skilled in the art, the present application can have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the technical ideas and principles of the present application should be included in the protection scope of the present application.
Claims
1. A process for producing an elastic nonwoven fabric, characterized in that: The following steps are involved: (1) Mixing and drying: 95 parts of TPU and 2 parts of a mixture of an ester antioxidant and an amine antioxidant are mixed and dried at a temperature of 100° C. for 3 hours, and then added into a mixer for mixing to obtain polymer chips, wherein the soft segment structure of the TPU is PBA, and the hard segment structure of the TPU is MDI; the Shore hardness of the TPU is 65D; (2) Melt extrusion: Place the polymer slices in a screw extruder, adjust the speed of the screw extruder to 250 r / min, the first zone of the screw extruder to 100°C, the second zone to 180°C, the third zone to 200°C, the fourth zone to 210°C, and the fifth zone to 220°C. The polymer slices are heated and melted in the screw extruder to form a viscous melt, which is compressed by the extruder and transported to the melt pipe; (3) Filtration: The melt is extruded and transported to the filter, where impurities and unmelted particles are filtered out through the filter; (4) Metering: The filtered melt flows through a metering pump, and the pressure of the metering pump is adjusted to 32 MPa to continuously and stably transport the filtered melt into the spinning machine; (5) Spinning into a web: The die temperature is set to 220°C for the first zone, 230°C for the second zone, 240°C for the third zone, and 250°C for the fourth zone. After the melt enters the die and is mixed evenly, it is evenly distributed in each spinning hole of the spinneret, and a thin stream is evenly ejected from the spinning hole. Finally, short fibers are formed by hot air traction with a wind pressure of 18 MPa and a temperature of 250°C. The short fibers are webbed on a mesh curtain, and the distance between the die and the mesh curtain is 30 cm. (6) Cooling: After the web is formed, it is further cooled by a cold air system to obtain a fabric sample; (7) Stretching and winding: Winding the cooled fabric sample at a speed of 18 m / min; Or include the following steps: (1) Mixing and drying: 100 parts of TPU and 1.2 parts of a mixture of an ester antioxidant and a phenolic antioxidant are mixed and dried at a temperature of 90°C for 3 hours, and added into a mixer for mixing to obtain polymer chips, wherein the soft segment structure of TPU is a bio-based polyol, and the hard segment structure of TPU is NDI; the Shore hardness of TPU is 70D; (2) Melt extrusion: Place the polymer slices into a screw extruder, adjust the speed of the screw extruder to 170r / min, the first zone of the screw extruder to 110°C, the second zone to 150°C, the third zone to 200°C, the fourth zone: 210°C, and the fifth zone to 240°C. The polymer slices are heated and melted in the screw extruder to form a viscous melt, which is compressed by the extruder and transported to the melt pipe; (3) Filtration: The melt is extruded and transported to the filter, where impurities and unmelted particles are filtered out through the filter; (4) Metering: The filtered melt flows through the metering pump, and the pressure of the metering pump is adjusted to 20 MPa to continuously and stably transport the filtered melt into the spinning machine; (5) Spinning into a web: The die temperature is set to 210°C for the first zone, 220°C for the second zone, 240°C for the third zone, and 250°C for the fourth zone. After the melt enters the die and is mixed evenly, it is evenly distributed in each spinning hole of the spinneret, and a thin stream is evenly ejected from the spinning hole. Finally, short fibers are formed by hot air traction with a wind pressure of 24 MPa and a temperature of 270°C. The short fibers are webbed on a mesh curtain. The distance between the die and the mesh curtain is 40 cm. (6) Cooling: After forming the web, it is further cooled by a cold air system to obtain a fabric sample; (7) Stretching and winding: Wind the cooled fabric sample at a speed of 26 m / min.
2. An application of the elastic nonwoven fabric prepared by any one of the production processes described in claim 1 in shoe materials, clothing linings, medical dressings, menstrual pants, sanitary pants, and facial mask base fabrics.
Citation Information
Patent Citations
Preparation method of TPU / PLA melt-blown composite non-woven fabric
CN115387023A
Method and equipment for making elastic nonwovens from polyurethane by melting and jetting material to form mesh
CN1445390A
Fibers, particularly nonwoven fabric based on thermoplastic polyurethane
US20100248575A1
Melt-blown nonwoven fabric and hygienic material
WO2023190074A1