Flexible thin film devices and methods of making and using the same, wearable devices
By preparing SrBi4Sc1-xFexTi3O15-δ thin films on flexible substrates and fabricating interdigitated electrodes, the problem of existing sensors being inconvenient for wearable applications is solved, enabling integrated detection of optical and magnetic fields. This method has advantages such as being lightweight and flexible.
Patent Information
- Application Number
- CN202311501455.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-13
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-11-13
AI Technical Summary
Existing sensors for multiphysics environment detection are mostly large devices, which are not convenient enough. Improvements are needed to facilitate their application in wearable devices.
SrBi4Sc1-xFexTi3O15-δ thin films were prepared on flexible substrates using a sol-gel method combined with photolithography, and interdigitated electrodes were fabricated on them to achieve integrated detection of optical and magnetic fields.
The fabricated flexible thin-film devices are lightweight and flexible, and can exhibit sensitive responses under different physical field environments, making them suitable for wearable devices and achieving portability and flexibility.
Smart Images

Figure CN117558825B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of wearable devices, and more specifically, to flexible thin-film devices, their fabrication methods and applications, and wearable devices. Background Technology
[0002] With the development of wearable flexible devices, the practical applications of various thin-film devices have received widespread attention. Flexible electronic devices possess advantages such as good flexibility, portability, and the ability to be bent freely, and can be integrated with three-dimensional curved surfaces for application in the field of wearable electronics. The resistive memory, pain sensing system, and strain sensor designed and manufactured using this technology demonstrate the great application potential of flexible electronic devices in daily life. Existing sensors for multi-physics environment detection are mostly large devices, which are not convenient enough; further improvements in this area are anticipated. Summary of the Invention
[0003] This application provides a method for fabricating wearable thin-film devices for multi-physics environmental detection, primarily applied to the detection of ultraviolet light and magnetic fields that affect the human body. Wearable thin-film devices fabricated using this method possess advantages such as light weight, good flexibility, and ease of manufacturing, and can be applied in fields such as environmental monitoring and wearable flexible devices. Specifically, this application achieves the detection of light field wavelength and magnetic field strength, with a detectable wavelength range of 200nm to 600nm and a magnetic field range of 0oe to 1800oe. It exhibits different open-circuit voltage and short-circuit current responses to different external field conditions, integrating magneto-optical integrated detection.
[0004] This application provides a method for fabricating a flexible thin-film device, comprising the following steps:
[0005] Step 1: Deposit Pt as a buffer layer on a fluorine mica substrate, and then anneal it;
[0006] Step 2: Add bismuth nitrate, scandium acetate, strontium nitrate, ferric nitrate, and tetrabutyl titanate to an ethylene glycol solution, add acetylacetone, stir until clear, and then age to obtain the precursor solution;
[0007] Step 3: The precursor liquid is coated onto the buffer layer, baked and sintered in an oxygen atmosphere, and then naturally cooled.
[0008] Step 4: Repeat step 3 thirteen to fifteen times to perform multilayer coating, then sinter in an oxygen atmosphere, and after natural cooling, form SrBi4Sc on the buffer layer. 1-x Fe x Ti3O 15-δ Thin film, wherein x is 0.2, 0.4 or 0.6, and δ is 0.5;
[0009] Step 5: Apply photoresist to the SrBi4Sc1-x Fe x Ti3O 15-δ The thin film surface is then baked, and the photoresist is coated and baked two to four times to create a SrBi4Sc film coated with the photoresist. 1-x Fe x Ti3O 15-δ The thin film is aligned with the interdigitated electrode mask pattern and subjected to ultraviolet exposure and development, followed by baking;
[0010] Step 6: Deposit chromium as a transition layer on the developed photoresist, deposit gold on the transition layer, and then sonicate in an acetone solution to obtain a flexible thin film device with interdigitated electrodes.
[0011] In some embodiments, in step 1, a 150 nm thick Pt layer is deposited on the fluorine mica substrate as the buffer layer, and then annealed at 650 degrees Celsius for 5 minutes.
[0012] In some embodiments, in step 2, the molar ratio between bismuth nitrate, scandium acetate, strontium nitrate, ferric nitrate, and tetrabutyl titanate is 4:1-x:1:x:3. The above substances are added to an ethylene glycol solution, and 1 ml of acetylacetone is added. The mixture is stirred until clear and aged for 7 days to obtain the precursor solution.
[0013] In some embodiments, in step 3, coating the precursor liquid onto the buffer layer includes using 800 rpm and 5000 rpm for 10 s and 45 s respectively, followed by baking at 350 degrees Celsius for 5 minutes, then sintering at 700 degrees Celsius for 5 minutes in an oxygen atmosphere with a beam flow of 0.2 ml / min, and then natural cooling.
[0014] In some embodiments, in step 4, step 3 is repeated fourteen times, resulting in a total of 15 layers. The layers are then sintered at 700°C for 20 minutes in an oxygen atmosphere with a beam flow rate of 0.2 ml / min. After natural cooling, the SrBi4Sc layer is formed on the buffer layer. 1-x Fe x Ti3O 15-δ film.
[0015] In some embodiments, in step 5, positive photoresist is coated onto the SrBi4Sc 1-x Fe x Ti3O 15-δFor the thin film surface, the coating was applied at 500 rpm and 4000 rpm for 10 s and 35 s respectively, followed by baking at 100 degrees Celsius for 5 minutes. The positive photoresist was then applied and baked three times. The thin film coated with the positive photoresist was aligned with the interdigitated electrode mask pattern and exposed to ultraviolet light for 30 s, followed by development and baking at 100 degrees Celsius for 3 minutes.
[0016] In some embodiments, in step 6, chromium is deposited on the developed photoresist for 100 seconds as the transition layer, then gold is deposited on the transition layer for 300 seconds, and then ultrasonically vibrated in an acetone solution for 1 minute to obtain a flexible thin film device coated with interdigitated electrodes.
[0017] This application also provides a flexible thin film device obtained according to the above-described method for fabricating flexible thin film devices.
[0018] This application also provides the application of the above-mentioned flexible thin-film device in wearable devices for the detection of magnetic fields and / or optical fields.
[0019] This application also provides a wearable device, which includes the above-described flexible thin-film device.
[0020] This application utilizes the sol-gel method combined with photolithography to fabricate wearable thin-film devices for multi-physics environment detection. This method is simple to prepare and low in cost, and can achieve integrated magneto-optical detection, which has great application value. Attached Figure Description
[0021] Figure 1 This is a photograph of the thin film prepared in Example 1 of this application in its natural state.
[0022] Figure 2 This is a photograph of the thin film prepared in Example 1 of this application in a bent state.
[0023] Figure 3 This is a photograph of the thin-film device prepared in Example 1 of this application.
[0024] Figure 4 The SrBi4Sc prepared for this application 1-x Fe x Ti3O 15-δ XRD patterns of flexible thin films (x = 0.2, 0.4, 0.6, δ = 0.5).
[0025] Figure 5 The SrBi4Sc prepared for this application 0.8 Fe 0.2 Ti3O 15-δ IV response of flexible thin-film devices under different magnetic fields.
[0026] Figure 6 The SrBi4Sc prepared for this application 0.6 Fe 0.4 Ti3O 15-δ IV response of flexible thin-film devices under different magnetic fields.
[0027] Figure 7 The SrBi4Sc prepared for this application 0.4 Fe 0.6 Ti3O 15-δ IV response of flexible thin-film devices under different magnetic fields.
[0028] Figure 8 The SrBi4Sc prepared for this application 0.8 Fe 0.2 Ti3O 15-δ IV response of flexible thin-film devices under illumination of different wavelengths of light.
[0029] Figure 9 The SrBi4Sc prepared for this application 0.6 Fe 0.4 Ti3O 15-δ IV response of flexible thin-film devices under illumination of different wavelengths of light.
[0030] Figure 10 The SrBi4Sc prepared for this application 0.4 Fe 0.6 Ti3O 15-δ IV response of flexible thin-film devices under illumination of different wavelengths of light. Detailed Implementation
[0031] The following examples are intended to enable those skilled in the art to gain a more comprehensive understanding of this application, but do not limit this application in any way. Unless otherwise stated, all reagents used in this application are conventional commercially available reagents.
[0032] This application provides a method for fabricating flexible thin-film devices for detecting optical and magnetic fields. This method employs a sol-gel method, which is energy-efficient, easily industrialized, and low-cost. SrBi4Sc was fabricated on a flexible fluorinated mica substrate. 1-x Fe x Ti3O 15-δ Thin films (X = 0.2, 0.4, 0.6) with a wavelength of δ = 0.5 exhibited different sensitive responses under different magnetic fields and light fields of different wavelengths. After peeling, the films demonstrated good flexibility, making them suitable for applications in wearable devices.
[0033] The fabrication of wearable thin-film devices for multiphysics environment detection mainly involves three steps:
[0034] (1) A layer of Pt with a thickness of about 150 nm was deposited on a flexible substrate of fluorine crystal mica (F-mica) by plasma sputtering as a buffer layer.
[0035] (2) Using the sol-gel method, a clear SrBi4Sc solution was prepared. 1-x Fe x Ti3O 15-δ The solution was aged for 7 days, and then spin-coated uniformly onto the Pt / F-mica substrate surface using a spin coater at 800 rpm and 5000 rpm for 10 s and 45 s, respectively. The substrate was then baked at 350°C for 5 minutes. Subsequently, it was placed in a rapid annealing furnace and sintered at 700°C for 5 minutes, and the deposition process was repeated 15 times. Finally, it was sintered in a rapid annealing furnace at 700°C for 20 minutes to obtain SrBi4Sc. 1-x Fe x Ti3O 15-δ film;
[0036] (3) Interdigitated electrodes are fabricated on the thin film obtained in the previous step using photolithography to obtain a flexible thin film device for detecting light and magnetic fields.
[0037] Specifically, the fabrication method of a wearable thin-film device for multi-physics environment detection includes the following steps:
[0038] Step 1: A Pt layer of approximately 150 nm thickness was deposited on a fluorine mica substrate using a plasma sputtering apparatus as a buffer layer, and then annealed in a rapid annealing furnace at 650 degrees Celsius for 5 minutes. This buffer layer is beneficial for the crystallization and growth of the thin film.
[0039] Step 2: Add analytical grade bismuth nitrate, scandium acetate, strontium nitrate, ferric nitrate, and tetrabutyl titanate to an ethylene glycol solution in a molar ratio of 4:1 to x:1:x:3, and add 1 ml of acetylacetone. Stir until clear. Aging for 7 days to obtain the precursor solution.
[0040] Step 3: The solution obtained in Step 2 was dropped onto the surface of the Pt / F-mica substrate and spin-coated at 800 rpm and 5000 rpm for 10 s and 45 s respectively, followed by baking at 350 degrees Celsius for 5 minutes. Then it was placed in a rapid annealing furnace and sintered at 700 degrees Celsius for 5 minutes in an oxygen atmosphere with a beam flow of 0.2 ml / min, and then allowed to cool naturally.
[0041] Step 4: Repeat step 3, depositing 15 layers. Finally, place it in a rapid annealing furnace and sinter at 700 degrees Celsius for 20 minutes in an oxygen atmosphere with a beam flow rate of 0.2 ml / min. After natural cooling, a crystallized and high-performance SrBi4Sc is obtained. 1-x Fe x Ti3O 15-δ film.
[0042] Step 5: Spin-coat a positive photoresist (e.g., RZJ-304-25) onto the surface of the film obtained in the previous step using spin coating at 500 rpm and 4000 rpm for 10 s and 35 s respectively. Then bake at 100°C for 5 minutes, repeating this process three times to achieve a sufficient photoresist thickness (approximately 5 μm) for subsequent pattern transfer. Align the photoresist-coated film with the interdigitated electrode mask pattern and expose it to UV light for 30 s, followed by thorough development in a developer (e.g., RZX-3038). Finally, bake at 100°C for 3 minutes.
[0043] Step 6: Deposit chromium for 100 seconds as a transition layer (adhesion layer) (approximately 50 nm thick) by plasma sputtering, followed by gold deposition for 300 seconds (approximately 150 nm thick), and then ultrasonically vibrate the film in acetone solution for 1 minute to obtain a thin film device with interdigitated electrodes.
[0044] The following description, in conjunction with specific embodiments, will provide a better understanding of this application.
[0045] Example 1 SrBi4Sc 0.8 Fe 0.2 Ti3O 15-δ Fabrication of thin-film devices (δ=0.5)
[0046] Thin film devices were fabricated using the following raw materials (all of which are analytical grade with a purity of ≥99.9%), a spin coater, a rapid annealing furnace, and a photolithography machine.
[0047] The following describes the fabrication of a wearable SrBi4Sc for multiphysics environment detection. 0.8 Fe 0.2 Ti3O 15-δ Specific methods for thin-film devices:
[0048] 1.1): A Pt layer of approximately 150 nm thickness was deposited on a fluorinated mica (F-mica) substrate using a plasma sputtering apparatus as a buffer layer, and then placed in a rapid annealing furnace and annealed at 650 degrees Celsius for 5 minutes.
[0049] 1.2): Analytical grade 8 mmol bismuth nitrate, 1.6 mmol scandium acetate, 2 mmol strontium nitrate, 0.4 mmol ferric nitrate, and 6 mmol tetrabutyl titanate were added to ethylene glycol solution respectively. After dissolution, 1 ml acetylacetone was added, and the volume was adjusted to 20 ml with ethylene glycol solution to achieve a concentration of 0.1 mol / L. The solution was stirred until clear and aged for 7 days to obtain the precursor solution.
[0050] 1.3): The solution obtained in step 2 was dropped onto the surface of a Pt / F-mica substrate and spin-coated at 800 rpm and 5000 rpm for 10 s and 45 s respectively, followed by baking at 350 degrees Celsius for 5 minutes. Then it was placed in a rapid annealing furnace and sintered at 700 degrees Celsius for 5 minutes in an oxygen atmosphere with a beam flow of 0.2 ml / min, and then allowed to cool naturally.
[0051] 1.4): Repeat step 1.3, depositing 15 layers. Finally, place in a rapid annealing furnace and sinter at 700 degrees Celsius for 20 minutes in an oxygen atmosphere with a beam flow rate of 0.2 ml / min. After natural cooling, obtain SrBi4Sc with excellent crystallinity and properties. 0.8 Fe 0.2 Ti3O 15-δ (δ=0.5) thin film, Figure 4 Its XRD pattern is shown.
[0052] 1.5): Positive photoresist is dropped onto the surface of the film obtained in the previous step and spin-coated at 500 rpm and 4000 rpm for 10 s and 35 s respectively. Then, it is baked at 100 degrees Celsius for 5 minutes, repeated three times to achieve a certain thickness of photoresist for subsequent pattern transfer. The photoresist-coated film is aligned with the interdigitated electrode mask pattern (the mask consists of periodically arranged intersecting finger electrodes, with an adjacent finger electrode distance of 200 μm and each finger electrode width of 50 μm) and exposed to UV light for 30 s, followed by thorough development. Then, it is baked at 100 degrees Celsius for 3 minutes.
[0053] 1.6): A SrBi4Sc film with interdigitated electrodes was obtained by plasma sputtering to deposit chromium for 100 seconds as a transition layer (adhesion layer), followed by gold deposition for 300 seconds, and then ultrasonically vibrating the film in acetone solution for 1 minute. 0.8 Fe 0.2 Ti3O 15-δ Thin film devices.
[0054] Example 2 SrBi4Sc 0.6 Fe 0.4 Ti3O 15-δ Preparation of thin films (δ=0.5)
[0055] Thin film devices were fabricated using the following raw materials (all of which are analytical grade with a purity of ≥99.9%), a spin coater, a rapid annealing furnace, and a photolithography machine.
[0056] The following describes the fabrication of a wearable SrBi4Sc for multiphysics environment detection. 0.6 Fe 0.4 Ti3O 15-δ Specific methods for thin-film devices:
[0057] 1.1): A Pt layer of approximately 150 nm thickness was deposited on a fluorinated mica (F-mica) substrate using a plasma sputtering apparatus as a buffer layer, and then placed in a rapid annealing furnace and annealed at 650 degrees Celsius for 5 minutes.
[0058] 1.2): Analytical grade 8 mmol bismuth nitrate, 1.2 mmol scandium acetate, 2 mmol strontium nitrate, 0.8 mmol ferric nitrate, and 6 mmol tetrabutyl titanate were added to ethylene glycol solution respectively. After dissolution, 1 ml acetylacetone was added, and the volume was adjusted to 20 ml with ethylene glycol solution to achieve a concentration of 0.1 mol / L. The solution was stirred until clear and aged for 7 days to obtain the precursor solution.
[0059] 1.3): The solution obtained in step 2 was dropped onto the surface of a Pt / F-mica substrate and spin-coated at 800 rpm and 5000 rpm for 10 s and 45 s respectively, followed by baking at 350 degrees Celsius for 5 minutes. Then it was placed in a rapid annealing furnace and sintered at 700 degrees Celsius for 5 minutes in an oxygen atmosphere with a beam flow of 0.2 ml / min, and then allowed to cool naturally.
[0060] 1.4): Repeat step 3, depositing 15 layers. Finally, place in a rapid annealing furnace and sinter at 700 degrees Celsius for 20 minutes in an oxygen atmosphere with a beam flow rate of 0.2 ml / min. After natural cooling, obtain SrBi4Sc with excellent crystallinity and properties. 0.6 Fe 0.4 Ti3O 15-δ (δ=0.5) thin film, Figure 4 Its XRD pattern is shown.
[0061] 1.5): Positive photoresist is dropped onto the surface of the film obtained in the previous step and spin-coated at 500 rpm and 4000 rpm for 10 s and 35 s respectively. Then, it is baked at 100 degrees Celsius for 5 minutes, repeated three times to achieve a certain thickness of photoresist for subsequent pattern transfer. The photoresist-coated film is aligned with the interdigitated electrode mask pattern and exposed to ultraviolet light for 30 s, followed by thorough development. Then, it is baked at 100 degrees Celsius for 3 minutes.
[0062] 1.6): A SrBi4Sc film with interdigitated electrodes was obtained by plasma sputtering to deposit chromium for 100 seconds as a transition layer (adhesion layer), followed by gold deposition for 300 seconds, and then ultrasonically vibrating the film in acetone solution for 1 minute. 0.6 Fe 0.4 Ti3O 15-δ Thin film devices.
[0063] Example 3 SrBi4Sc 0.4 Fe 0.6 Ti3O 15-δ Preparation of thin films (δ=0.5)
[0064] Thin film devices were fabricated using the following raw materials (all of which are analytical grade with a purity of ≥99.9%), a spin coater, a rapid annealing furnace, and a photolithography machine.
[0065] The following describes the fabrication of a wearable SrBi4Sc for multiphysics environment detection. 0.4 Fe 0.6 Ti3O 15-δ Specific methods for thin-film devices:
[0066] 1.1): A Pt layer of approximately 150 nm thickness was deposited on a fluorinated mica (F-mica) substrate using a plasma sputtering apparatus as a buffer layer, and then placed in a rapid annealing furnace and annealed at 650 degrees Celsius for 5 minutes.
[0067] 1.2): Analytical grade 8 mmol bismuth nitrate, 0.8 mmol scandium acetate, 2 mmol strontium nitrate, 1.2 mmol ferric nitrate, and 6 mmol tetrabutyl titanate were added to ethylene glycol solution respectively. After dissolution, 1 ml acetylacetone was added, and the volume was adjusted to 20 ml with ethylene glycol solution to achieve a concentration of 0.1 mol / L. The solution was stirred until clear and aged for 7 days to obtain the precursor solution.
[0068] 1.3): The solution obtained in step 2 was dropped onto the surface of a Pt / F-mica substrate and spin-coated at 800 rpm and 5000 rpm for 10 s and 45 s respectively, followed by baking at 350 degrees Celsius for 5 minutes. Then it was placed in a rapid annealing furnace and sintered at 700 degrees Celsius for 5 minutes in an oxygen atmosphere with a beam flow of 0.2 ml / min, and then allowed to cool naturally.
[0069] 1.4): Repeat step 3, depositing 15 layers. Finally, place in a rapid annealing furnace and sinter at 700 degrees Celsius for 20 minutes in an oxygen atmosphere with a beam flow rate of 0.2 ml / min. After natural cooling, obtain SrBi4Sc with excellent crystallinity and properties. 0.4 Fe 0.6 Ti3O 15-δ (δ=0.5) thin film, Figure 4 Its XRD pattern is shown.
[0070] 1.5): Positive photoresist is dropped onto the surface of the film obtained in the previous step and spin-coated at 500 rpm and 4000 rpm for 10 s and 35 s respectively. Then, it is baked at 100 degrees Celsius for 5 minutes, repeated three times to achieve a certain thickness of photoresist for subsequent pattern transfer. The photoresist-coated film is aligned with the interdigitated electrode mask pattern and exposed to ultraviolet light for 30 s, followed by thorough development. Then, it is baked at 100 degrees Celsius for 3 minutes.
[0071] 1.6): A SrBi4Sc film with interdigitated electrodes was obtained by plasma sputtering to deposit chromium for 100 seconds as a transition layer (adhesion layer), followed by gold deposition for 300 seconds, and then ultrasonically vibrating the film in acetone solution for 1 minute. 0.4 Fe 0.6 Ti3O 15-δ Thin film devices.
[0072] Figure 1 This is a photograph of the thin film prepared in Example 1 of this application in its natural state. Figure 2 This is a photograph of the thin film prepared in Example 1 of this application in a bent state. Figure 3 This is a photograph of the thin-film device prepared in Example 1 of this application. Figure 4 The SrBi4Sc prepared for this application 1-x Fe x Ti3O 15-δ XRD patterns of flexible thin films (x = 0.2, 0.4, 0.6). Figure 5 The SrBi4Sc prepared for this application 0.8 Fe 0.2 Ti3O 15-δ IV response of flexible thin-film devices under different magnetic fields. Figure 6 The SrBi4Sc prepared for this application 0.6 Fe 0.4 Ti3O 15-δ IV response of flexible thin-film devices under different magnetic fields. Figure 7 The SrBi4Sc prepared for this application 0.4 Fe 0.6 Ti3O 15-δ IV response of flexible thin-film devices under different magnetic fields. Figure 8 The SrBi4Sc prepared for this application 0.8 Fe 0.2 Ti3O 15-δ IV response of flexible thin-film devices under illumination of different wavelengths of light. Figure 9 The SrBi4Sc prepared for this application 0.6 Fe 0.4 Ti3O 15-δ IV response of flexible thin-film devices under illumination of different wavelengths of light. Figure 10 The SrBi4Sc prepared for this application 0.4 Fe 0.6 Ti3O 15-δ IV response of flexible thin-film devices under illumination of different wavelengths of light. For example... Figure 2 As shown, the film prepared in this application has better flexibility.
[0073] like Figures 5 to 10As shown in Figure IV, the thin film device prepared in this application has a sensitive response to the applied magnetic field and optical field. As the applied magnetic field increases, the open-circuit voltage and short-circuit current of the thin film device gradually increase. Under the condition of applied optical field, as the wavelength of light increases, the open-circuit voltage and short-circuit current of the thin film device show a phenomenon of first increasing and then decreasing, and exhibiting the maximum value near the spectral response wavelength of the thin film.
[0074] This application utilizes the sol-gel method combined with micro / nano lithography to achieve multi-physics environment detection functionality, and integrates it onto a flexible substrate, exhibiting excellent flexibility and applicability in the field of smart wearable devices. This application fabricates SrBi4Sc... 1- x Fe x Ti3O 15-δ A flexible thin film was fabricated with interdigitated electrodes, and sensitive response outputs were obtained under varying optical and magnetic field conditions. Therefore, this application can realize the detection of optical and magnetic fields in a low-cost and easy-to-fabricate manner, and the device has advantages such as light weight, small size, and high flexibility.
[0075] The wearable thin-film device prepared in this application for multi-physics field environmental detection can be applied to the detection of ultraviolet light fields and magnetic fields in daily life. It has advantages such as good flexibility, portability, and the ability to be freely bent. It can be integrated with three-dimensional curved surfaces and applied in the field of wearable electronic devices, with great industrial application and commercial prospects.
[0076] Those skilled in the art should understand that the above embodiments are merely exemplary embodiments, and various changes, substitutions, and modifications can be made without departing from the spirit and scope of this application.
Claims
1. A method for fabricating a flexible thin-film device, characterized in that, Includes the following steps: Step 1: Deposit Pt as a buffer layer on a fluorine mica substrate, and then anneal it; Step 2: Add bismuth nitrate, scandium acetate, strontium nitrate, ferric nitrate, and tetrabutyl titanate to an ethylene glycol solution, add acetylacetone, stir until clear, and then age to obtain the precursor solution; Step 3: The precursor liquid is coated onto the buffer layer, baked and sintered in an oxygen atmosphere, and then naturally cooled. Step 4: Repeat step 3 thirteen to fifteen times to perform multilayer coating, then sinter in an oxygen atmosphere, and after natural cooling, form SrBi4Sc on the buffer layer. 1-x Fe x Ti3O 15-δ Thin film, wherein x is 0.2, 0.4 or 0.6, and δ is 0.5; Step 5: Apply photoresist to the SrBi4Sc 1-x Fe x Ti3O 15-δ The thin film surface is then baked, and the photoresist coating and baking process is repeated two to four times to coat the SrBi4Sc with the photoresist. 1-x Fe x Ti3O 15-δ The thin film is aligned with the interdigitated electrode mask pattern and subjected to ultraviolet exposure and development, followed by baking; Step 6: Deposit chromium as a transition layer on the developed photoresist, deposit gold on the transition layer, and then sonicate in an acetone solution to obtain a flexible thin film device with interdigitated electrodes.
2. The method for fabricating a flexible thin-film device according to claim 1, characterized in that, In step 1, a 150 nm thick Pt layer is deposited on the fluorine mica substrate as the buffer layer, and then annealed at 650 degrees Celsius for 5 minutes.
3. The method for fabricating a flexible thin-film device according to claim 1, characterized in that, In step 2, the molar ratio of bismuth nitrate, scandium acetate, strontium nitrate, ferric nitrate, and tetrabutyl titanate is 4:1-x:1:x:
3. The above substances are added to an ethylene glycol solution, and 1 ml of acetylacetone is added. The mixture is stirred until clear and aged for 7 days to obtain the precursor solution.
4. The method for fabricating a flexible thin-film device according to claim 1, characterized in that, In step 3, the precursor liquid is coated onto the buffer layer at 800 rpm and 5000 rpm, homogenized for 10 s and 45 s respectively, then baked at 350 degrees Celsius for 5 minutes, and then sintered at 700 degrees Celsius for 5 minutes in an oxygen atmosphere with a beam flow rate of 0.2 ml / min, and then naturally cooled.
5. The method for fabricating a flexible thin-film device according to claim 1, characterized in that, In step 4, step 3 is repeated fourteen times, resulting in a total of 15 layers. The film is then sintered at 700°C for 20 minutes in an oxygen atmosphere with a beam flow rate of 0.2 ml / min. After natural cooling, the SrBi4Sc film is formed on the buffer layer. 1-x Fe x Ti3O 15-δ film.
6. The method for fabricating a flexible thin-film device according to claim 1, characterized in that, In step 5, positive photoresist is coated onto the SrBi4Sc. 1-x Fe x Ti3O 15-δ For the thin film surface, the coating was applied at 500 rpm and 4000 rpm for 10 s and 35 s respectively, followed by baking at 100 degrees Celsius for 5 minutes. The positive photoresist was then applied and baked three times. The thin film coated with the positive photoresist was aligned with the interdigitated electrode mask pattern and exposed to ultraviolet light for 30 s, followed by development and baking at 100 degrees Celsius for 3 minutes.
7. The method for fabricating a flexible thin-film device according to claim 1, characterized in that, In step 6, chromium is deposited on the developed photoresist for 100 seconds as the transition layer, then gold is deposited on the transition layer for 300 seconds, and then ultrasonically vibrated in acetone solution for 1 minute to obtain a flexible thin film device coated with interdigitated electrodes.
8. The flexible thin film device obtained by the method for preparing the flexible thin film device according to any one of claims 1 to 7.
9. The application of the flexible thin-film device according to claim 8 in a wearable device for detecting magnetic fields and / or optical fields.
10. A wearable device, characterized in that, The wearable device includes the flexible thin-film device according to claim 8.
Citation Information
Patent Citations
Preparation method of flexible ferroelectric photovoltaic field effect transistor based on black phosphorus two-dimensional semiconductor
CN110224025A
Composition for ferroelectric thin film formation, method for forming ferroelectric thin film, and ferroelectric thin film formed by the method thereof
US20110098173A1