A method for regulating hydroxyl groups on the surface of a silica carrier for the preparation of a catalyst for the synthesis of methyl methacrylate
By systematically regulating the silicon hydroxyl groups on the surface of the silica carrier and loading acid and alkali active components, the problem of low activity and carbon deposition of existing catalysts has been solved, and efficient catalyst preparation and simplified processes have been achieved, making it suitable for large-scale production.
Patent Information
- Application Number
- CN202311528877.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-16
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-11-16
AI Technical Summary
In the existing technology, supported solid catalysts have low activity, severe carbon deposition, short regeneration cycle, complicated modification steps and are not suitable for large-scale production in the aldol condensation reaction.
By systematically regulating the silanol groups on the surface of the silica carrier, a modified carrier is prepared, and Sm and Cs are loaded on it as acid-base active components. The methyl methacrylate catalyst is synthesized through a one-step method, using porous silica. Balls and specific temperature rise roasting procedures improve catalytic activity.
It improves the activity and durability of the catalyst, simplifies the processing steps, is suitable for large-scale production, provides a suitable number of silanol groups, reduces the formation of clusters of active components, and extends the service life of the catalyst.
Abstract
Description
Technical Field
[0001] The present invention relates to a method for systematically regulating hydroxyl groups on the surface of a silicon carrier. The treated carrier can be used to prepare a Cs-based catalyst for an aldol condensation reaction, i.e., synthesizing methyl methacrylate from methyl propionate and formaldehyde. The method has a high degree of treatment of hydroxyl groups on the surface of silicon dioxide. The use of the treated carrier to prepare an acid-base bifunctional catalyst required for the aldol condensation reaction can effectively improve the catalytic activity. The treatment method provided by the present invention is simple and easy to operate. Background Art
[0002] Methyl methacrylate (MMA) is an important organic chemical raw material with a wide range of uses. The leading methods for producing MMA in industry include the acetone cyanohydrin method (ACH), the C1 method, the C4 two-step oxidation method, the ethylene method, the coal-based method, etc. Among them, the coal-based route uses methyl acetate and formaldehyde as raw materials, generates methyl propionate after hydrogenation, and then reacts with formaldehyde on a solid catalyst to obtain methyl methacrylate through a gas-phase aldol condensation reaction. Compared with the traditional method, it is more environmentally friendly. However, the catalysts commonly used in the aldol condensation reaction, especially the supported solid catalysts, still have problems such as low activity, severe carbon deposition, and short regeneration cycle.
[0003] The activity of supported catalysts generally depends on the particle size and dispersion of the active components. Using a suitable carrier can not only increase the specific surface area of the catalyst and micronize the active components, but also improve the catalyst's resistance to toxicity, heat resistance, and carbon deposition, thereby extending its service life.
[0004] Silicon dioxide has become an important carrier material due to its high hydrothermal stability, controllable morphology and high surface area. There are a large number of silanol groups on its surface, and their types and quantities have different catalytic effects on different reactions. Therefore, the silica carrier needs to be modified for different reactions. CN20210355050 discloses a chemical modification method of silicon dioxide, in which the silanol groups on the surface of silicon dioxide are replaced by a silane coupling agent, tridecafluorooctane triethoxy, so as to improve the dispersibility, compatibility and stability of silicon dioxide in solvents. CN202210147224 uses inorganic acid, alcohol, ammonia and coating agent as raw materials, and uses a coating method to modify silicon dioxide. The above method uses hydrophobic silanization agents and other substances for modification. Although this can regulate the number of surface hydroxyl groups, it is not suitable for further large-scale catalyst production because the reagents used for modification are usually expensive and the processing steps are complicated. Summary of the invention
[0005] Based on the above problems, the purpose of the present invention is to provide a method for systematically regulating the hydroxyl groups on the surface of a silicon carrier, and to prepare a catalyst using a modified silica carrier for the one-step synthesis of methyl methacrylate from methyl propionate and formaldehyde.
[0006] A method for regulating the surface hydroxyl groups of a silica carrier for synthesizing a Cs-based catalyst for methyl methacrylate comprises the following steps:
[0007] a) preparing a modified silica carrier;
[0008] b) Weigh a certain amount of the salts of the active components Sm and Cs and place them in a blue-capped bottle, and add deionized water to prepare a salt solution;
[0009] c) adding the carrier obtained in step a) to the salt solution containing the active ingredient prepared in step b), allowing to stand for 5-24 hours and then drying in an oven at 50-100° C. for 3-6 hours;
[0010] d) placing the Sm, Cs precursor catalyst obtained in step c) in a muffle furnace, calcining at 500° C. for 3-12 h according to a certain heating program, and then naturally cooling to room temperature to obtain the catalyst.
[0011] The carrier in the method is porous silica spheres with a particle size of 2-5 mm and a maximum pore size of 2-10 nm;
[0012] The loading amount of the active component is based on the mass of the carrier and is calculated based on the mass of the oxide of the active component. The preferred loading amount of Cs is 1-10%, and the preferred loading amount of the Sm active component is 3-5%;
[0013] In the method, the active components Cs and Sm salts are mainly derived from one or more combinations of cesium nitrate, cesium carbonate, cesium acetate, cesium hydroxide, samarium nitrate, samarium chloride, and samarium sulfate;
[0014] Compared with the existing technology for preparing catalysts, the beneficial effects of the present invention are:
[0015] Before preparing the catalyst, the silica carrier is first modified, and the silanol content on the carrier surface is systematically regulated. The silanol content on the modified carrier surface reaches the optimal amount required for preparing the next step of the catalyst. Sm and Cs are added as acid-base active components to be loaded on the modified silicon carrier, which can make the catalyst have better activity. This method can provide a suitable number of silanols, reduce the possibility of clustering of active components, and improve catalytic activity. In addition, this method is simple, short in steps, and suitable for large-scale preparation of subsequent catalysts. DETAILED DESCRIPTION
[0016] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.
[0017] Determination of silanol content: Titration method is used to determine the content of silanol. The specific steps are as follows: weigh 2g of sample and put it into a 200mL beaker, add 25mL of anhydrous ethanol, and then add 75mL of 20% NaCl solution. After shaking, add the prepared HCl to adjust the pH to 4, and then slowly add NaOH solution to adjust the pH to 9. After maintaining for a certain period of time, record the amount of NaOH solution added to different samples. Finally, according to the following formula: N = (C*V*N A ) / S*m to calculate the content of surface silanol groups. The results of different embodiments are shown in Table 1.
[0018] Catalytic performance test: In a fixed bed microreactor, 3 g of catalyst was loaded into the reactor, where the molar ratio of methyl propionate / formaldehyde was 1 / 1, methyl propionate / methanol was 1 / 2, and the feed space velocity was 0.6 h -1 , the reaction temperature was 360°C, and the evaluation results are shown in Table 2.
[0019] Example 1
[0020] Take an appropriate amount of ethanolamine acetate in a beaker, and then place it in an oil bath at a set temperature for stirring. Then weigh 10g of silica carrier and add it to the ethanolamine acetate and stir at the required temperature for 1h. The beaker is open during the whole process and the oil bath temperature is maintained at 100℃. After the treatment, the solid product is collected by centrifugation, dried at 120℃ for 6h, and finally calcined at 500℃ for 4h, and the treated carrier is obtained after tableting;
[0021] Example 2
[0022] Take an appropriate amount of ethanolamine acetate in a beaker, and then place it in an oil bath at a set temperature for stirring. Then weigh 10g of silica carrier and add it to the ethanolamine acetate and stir at the required temperature for 3h. The beaker is open during the whole process and the oil bath temperature is maintained at 120℃. After the treatment, the solid product is collected by centrifugation, dried at 120℃ for 6h, and finally calcined at 500℃ for 4h, and the treated carrier is obtained after tableting;
[0023] Example 3
[0024] Weigh 10g of silica carrier into a crucible, and then put it into the reaction chamber for pulse roasting. In this process, a two-step roasting program is selected. In the first step, the pulse signal frequency is regulated by the controller. At a frequency of 200 Hz and a duration of 100 milliseconds each time, it is heated to 500°C for 3 hours, and then the frequency of the pulse signal is increased to keep it at 800°C for 5 hours. After the pulse roasting treatment is completed, the silica carrier is sealed and naturally cooled to obtain a pulse roasted carrier;
[0025] Example 4
[0026] Weigh 10g of silica carrier and put it into a three-necked flask, add 30mL of 5% peroxide and ammonia water, mix them and stir them in an oil bath at a constant temperature of 100°C for 5h, ensure condensation and reflux during the treatment process and have an outlet for releasing decomposition gas, and dry the obtained carrier in a drying oven at a constant temperature of 50°C for 3h.
[0027] obtaining a peroxide-treated carrier;
[0028] Example 5
[0029] Weigh 10 g of a silica carrier and perform the ion thermal treatment in Example 1, and then perform the pulse roasting treatment in Example 3 to obtain a silica carrier after the double treatment;
[0030] Example 6
[0031] (1) accurately weighing 0.21 g of samarium nitrate and 0.21 g of cesium nitrate, adding a certain amount of deionized water to fully dissolve them to obtain an aqueous solution containing samarium and cesium;
[0032] (2) The silica carrier obtained in Example (1) was added to the above solution and allowed to stand for 12 h. The solution was then dried at 120° C. for 12 h and calcined at 500° C. in a muffle furnace for 4 h. The catalyst was obtained after cooling.
[0033] Example 7
[0034] (1) Accurately weigh 0.40 g of samarium nitrate and 0.42 g of cesium nitrate, add a certain amount of deionized water to fully dissolve them to obtain an aqueous solution containing samarium and cesium;
[0035] (2) The silica carrier obtained in Example (2) was added to the above solution and allowed to stand for 12 h. The solution was then dried at 120° C. for 12 h and calcined at 500° C. in a muffle furnace for 4 h. The catalyst was obtained after cooling.
[0036] Example 8
[0037] (1) Accurately weigh 0.35 g of samarium sulfate and 0.42 g of cesium nitrate, add a certain amount of deionized water to fully dissolve them to obtain an aqueous solution containing samarium and cesium;
[0038] (2) The silica carrier obtained in Example (3) was added to the above solution and allowed to stand for 12 h. The solution was then dried at 120° C. for 12 h and calcined at 500° C. in a muffle furnace for 4 h. The catalyst was obtained after cooling.
[0039] Example 9
[0040] (1) Accurately weigh 0.19 g of samarium nitrate and 0.42 g of cesium nitrate, add a certain amount of deionized water to fully dissolve them to obtain an aqueous solution containing samarium and cesium;
[0041] (2) The silica carrier obtained in Example (4) was added to the above solution and allowed to stand for 12 h. The solution was then dried at 120° C. for 12 h and calcined at 500° C. in a muffle furnace for 4 h. The catalyst was obtained after cooling.
[0042] Example 10
[0043] (1) Accurately weigh 0.28 g of samarium nitrate and 0.42 g of cesium carbonate, add a certain amount of deionized water to fully dissolve them to obtain an aqueous solution containing samarium and cesium;
[0044] (2) The silica carrier obtained in Example (5) was added to the above solution and allowed to stand for 12 h. The solution was then dried at 120° C. for 12 h and calcined at 500° C. in a muffle furnace for 4 h. The catalyst was obtained after cooling.
[0045] Comparative Example
[0046] (1) Directly weigh 10 g of untreated silica support;
[0047] (2) The catalyst was prepared in the same manner as in Example 6, except that the untreated silica carrier described in (1) was selected as the carrier.
[0048] Table 1 Surface hydroxyl content of silicon carrier in different embodiments
[0049] Example <![CDATA[Silanol group content on the support (number / nm 2 )]]> Comparative Example 1.01 1 1.02 2 0.99 3 0.94 4 1.13 5 0.96
[0050] Table 2 Catalyst activity evaluation results
[0051] Example Methyl propionate conversion rate (%) MMA selectivity (%) Comparative Example 16.51 61.46 6 20.67 62.08 7 19.35 64.36 8 18.63 63.41 9 24.51 76.10 10 18.83 65.87
[0052] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for regulating hydroxyl groups on the surface of a silica carrier is applied to the preparation of a catalyst for synthesizing methyl methacrylate. Features The method includes the following: Ionic thermal treatment: Take an appropriate amount of ethanolamine acetate in a beaker, and then place it in an oil bath at a set temperature for stirring. Then weigh a certain mass of silica carrier and add it to the above oil bath. Keep the oil bath temperature at 120°C and stir for 1-3 hours or keep the oil bath temperature at 100°C and stir for 1 hour. After the treatment, collect the solid product by centrifugation, dry it at 120°C for 6 hours, and finally calcine it at 500°C for 4 hours. After tableting, the treated carrier is obtained.
Citation Information
Patent Citations
Heat energy recovery internal combustion engine
CN114508413A
Method for preparing polyaniline graft-modified silicon dioxide composite electrode material for supercapacitors
CN106565971A
Catalyst and process for production of ethylenically unsaturated carboxylic acids or esters
CN111344059A
Acid-base bifunctional catalyst for synthesizing methyl acrylate from methyl acetate and formaldehyde and preparation method of acid-base bifunctional catalyst
CN112774658A
Oxide layer forming method and semiconductor structure
CN114334627A