High-strength interior wall ceramic brick and preparation method thereof

By using clay and other raw materials and modified oxide powder preparation methods, combined with wet ball milling technology, internal defects and pore problems caused by improper selection of raw materials in ceramic tiles are solved, significantly improving the bending strength and density of ceramic tiles, satisfying the satisfaction of The market demand for improving the performance of ceramic tile.

CN117567133BActive Publication Date: 2024-11-19PINGXIANG LVBAO TECH GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311604218.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-28
Publication Date
2024-11-19
Estimated Expiration
2043-11-28

AI Technical Summary

Technical Problem

Improper raw material selection of existing ceramic tiles leads to insolid bonding between particles, prone to internal defects and tiny pores, affecting their mechanical properties and durability, and failing to meet the market's demand for improving the performance of ceramic tiles.

Method used

Using clay, potassium feldspar powder, modified oxide powder, diboron trioxide, zirconia, yttrium oxide, titanium carbide, quartz stone powder, calcium hydroxyphosphate powder and barium carbonate, the preparation method of specific modified oxide powder is carried out. With the wet ball milling process, high-strength inner wall ceramic tiles are formed to improve the bending strength and density of ceramic tiles.

Benefits of technology

It significantly improves the bending strength and mechanical properties of ceramic tiles, reduces water absorption, reduces defects and holes, improves the durability and density of ceramic tiles, and meets the market's demand for improving the performance of ceramic tiles.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-strength interior wall ceramic tile, the raw materials of which include: clay, potassium feldspar powder, modified oxide powder, boron trioxide, zirconium oxide, yttrium oxide, titanium carbide, quartz powder, hydroxy calcium phosphate powder and barium carbonate; the interior wall ceramic tile prepared by the method of the invention has high bending strength, excellent mechanical properties, low water absorption, dense structure, fewer defects and holes, and significantly improves the durability of the ceramic tile.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic materials, and in particular to a high-strength interior wall ceramic tile and a preparation method thereof. Background Art

[0002] Ceramic tiles are plate-shaped or block-shaped ceramic products made of clay and other inorganic non-metallic raw materials through molding, sintering and other processes. They are used to decorate and protect the walls and floors of buildings and structures. The raw materials used in the production of ordinary ceramic tiles are poorly selected, and the particles are not firmly bonded, which easily causes defects and many tiny pores in the ceramics. With the development of people's needs and the market, people continue to put forward new requirements for the performance of ceramic tiles. In order to meet the needs of the market, improving the mechanical properties and durability of ceramic tiles has become a hot spot for research and development by experts in major ceramic factories. In addition, improving the strength of ceramic tiles is conducive to reducing the thickness of ceramic tiles under the same use environment, promoting the thinning of ceramic tiles, effectively improving and alleviating the resource and energy consumption problems in the ceramic tile industry, and meeting the needs of energy conservation and emission reduction. Summary of the invention

[0003] To this end, the present invention provides a high-strength interior wall ceramic tile, the raw materials of which include: clay, potassium feldspar powder, modified oxide powder, boron trioxide, zirconium oxide, yttrium oxide, titanium carbide, quartz powder, hydroxy calcium phosphate powder and barium carbonate; the preparation method of the modified oxide powder is:

[0004] (1) preparing an aqueous solution of zinc nitrate in a reaction kettle, stirring the aqueous solution of zinc nitrate, then adding hexamethylenetetramine to the solution under stirring, continuing to stir the solution for more than 10 minutes after the addition is completed, then adding ammonium dihydrogen phosphate to the solution under stirring, adding sodium hydroxide solution after the addition is completed, then sealing the reaction kettle, heating to 120±3° C., keeping the temperature for more than 30 minutes, then air cooling to room temperature, opening the reaction kettle, separating the solid and liquid, washing the solid phase with deionized water, and drying to obtain a solid phase A;

[0005] (2) preparing an aqueous solution of lithium hydroxide; dispersing the solid phase A in ethanol to form a dispersion, stirring the dispersion, and then adding aluminum isopropoxide to the dispersion under stirring. After the addition is completed, the dispersion is stirred in a water bath at a constant temperature of 50±3°C for more than 50 minutes, and then the dispersion is spread in a glass dish and dried at 85°C to remove the ethanol; the dried solid phase is calcined at 500°C for more than 1 hour in an argon atmosphere, and then cooled to room temperature in an argon atmosphere to obtain an aluminum oxide coated powder; the aluminum oxide coated powder is immersed in the aqueous solution of lithium hydroxide for 4 to 5 minutes, and then the solid and liquid are separated, and the solid phase is calcined at 500°C for more than 1 hour to obtain a solid phase B;

[0006] (3) preparing a mixture of the solid phase B, pentafluoropyridine, ethylene glycol, ethanol and deionized water in a reactor, and preparing an ethanol solution of tetrabutyl titanate; stirring the mixture, and adding the ethanol solution of tetrabutyl titanate to the mixture under stirring. After the addition is completed, the reactor is closed, heated to 110° C. and kept warm for more than 8 hours, and then air-cooled to room temperature, the reactor is opened, the solid-liquid separation is carried out, the solid phase is washed with ethanol for more than 3 times, and then washed with deionized water for more than 3 times, and dried to obtain the modified oxide powder.

[0007] Furthermore, the raw material components are calculated by weight as follows: 50 parts of clay, 20-30 parts of potassium feldspar powder, 10-16 parts of modified oxide powder, 8-10 parts of boron trioxide, 3-5 parts of zirconium oxide, 3-5 parts of yttrium oxide, 4-9 parts of titanium carbide, 10-14 parts of quartz powder, 3-6 parts of hydroxy calcium phosphate powder, and 2-3 parts of barium carbonate; each raw material component is a sieved powder passing through a 300-mesh sieve.

[0008] Furthermore, in the step (1), in the aqueous solution of zinc nitrate, the concentration of zinc nitrate is 0.03-0.04 mol / L, and the solvent is water; the mass ratio of hexamethylenetetramine added to the solution is hexamethylenetetramine: solution = 4-5 g: 1 L; the amount ratio of ammonium dihydrogen phosphate added to the solution is ammonium dihydrogen phosphate: solution = 7-10 g: 1 L; in the sodium hydroxide solution, the mass percentage of sodium hydroxide is 10%, and the solvent is water; the ratio of the added volume of the sodium hydroxide solution to the volume of the solution added thereto is sodium hydroxide solution: solution = 2-4:10.

[0009] Furthermore, in the step (2), the concentration of lithium hydroxide in the aqueous solution of lithium hydroxide is 20 g / L, and the solvent is water; the solid-liquid mass ratio of the solid phase A dispersed in ethanol to form a dispersion is solid / liquid = 1:30; the mass ratio of aluminum isopropoxide added to the dispersion to the mass ratio of solid phase A in the dispersion is aluminum isopropoxide: solid phase A = 5 to 8:1.

[0010] Furthermore, in the step (2), the aluminum oxide coated powder is immersed in the aqueous solution of lithium hydroxide at a solid-liquid mass ratio of solid / liquid = 1:80.

[0011] Furthermore, in the step (3), the mass ratio of the solid phase B, pentafluoropyridine, ethylene glycol, ethanol and deionized water is solid phase B: pentafluoropyridine: ethylene glycol: ethanol: deionized water = 1: 0.4-0.6: 3-5: 50-60: 16-18; in the ethanol solution of tetrabutyl titanate, the mass percentage of tetrabutyl titanate is 20%, and the mass ratio of the ethanol solution of tetrabutyl titanate added to the mixed solution to the mass ratio of the solid phase B in the mixed solution is ethanol solution of tetrabutyl titanate: solid phase B = 20:1.

[0012] The present invention also discloses a method for preparing the interior wall ceramic tile, the steps comprising:

[0013] Step 1, weighing each raw material component according to the weight proportion, mixing the raw materials, adding water to wet-mill the mixture, and obtaining a slurry;

[0014] Step 2: spray granulate the slurry to obtain powder, and adjust the water content of the powder to 5wt%; press the powder into shape, and burn it to obtain the interior wall ceramic tile.

[0015] Furthermore, the wet ball milling process is as follows: the mass ratio of material, ball and water is material: ball: water = 1:1.5:1; the ball milling speed is 120r / min, and the ball milling time is 8h; the pressing molding pressure is 60MPa; the firing temperature is 1200°C, and the firing time is 2h. After the firing is completed, the ceramic bricks are cooled to room temperature with the furnace.

[0016] The beneficial effects of the present invention are that the interior wall ceramic tiles prepared by the method of the present invention have high bending strength, excellent mechanical properties, low water absorption, dense structure, fewer defects and holes, and significantly improve the durability of the ceramic tiles. DETAILED DESCRIPTION

[0017] The present invention will be further described below in conjunction with the embodiments.

[0018] Example 1

[0019] A high-strength interior wall ceramic tile, comprising raw materials: clay, potassium feldspar powder, modified oxide powder, boron trioxide, zirconium oxide, yttrium oxide, titanium carbide, quartz powder, hydroxy calcium phosphate powder and barium carbonate; the raw material components are calculated by weight as follows: 50 parts of clay, 20 parts of potassium feldspar powder, 10 parts of modified oxide powder, 8 parts of boron trioxide, 3 parts of zirconium oxide, 3 parts of yttrium oxide, 4 parts of titanium carbide, 10 parts of quartz powder, 3 parts of hydroxy calcium phosphate powder and 2 parts of barium carbonate; each raw material component is a sieved powder passing through a 300-mesh sieve; the preparation method of the modified oxide powder is as follows:

[0020] (1) A zinc nitrate aqueous solution is prepared in a reaction kettle, wherein the concentration of zinc nitrate in the zinc nitrate aqueous solution is 0.03 mol / L, and the solvent is water; the zinc nitrate aqueous solution is stirred, and then hexamethylenetetramine is added to the solution under stirring, and the mass ratio of hexamethylenetetramine added to the solution is hexamethylenetetramine: solution = 4 g: 1 L; after the addition is completed, the solution is stirred for 10 minutes, and then ammonium dihydrogen phosphate is added to the solution under stirring, and the amount ratio of ammonium dihydrogen phosphate added to the solution is ammonium dihydrogen phosphate: solution = 7 g: 1 L; after the addition is completed, a sodium hydroxide solution is added, wherein the mass percentage of sodium hydroxide in the sodium hydroxide solution is 10%, and the solvent is water; the ratio of the added volume of the sodium hydroxide solution to the volume of the solution added thereto is sodium hydroxide solution: solution = 2:10; then the reaction kettle is closed, heated to 120±3° C., kept warm for 30 minutes, and then air-cooled to room temperature, the reaction kettle is opened, the solid-liquid separation is carried out, the solid phase is washed 3 times with deionized water, and dried to obtain a solid phase A;

[0021] (2) preparing an aqueous solution of lithium hydroxide; in the aqueous solution of lithium hydroxide, the concentration of lithium hydroxide is 20 g / L, and the solvent is water; dispersing the solid phase A in ethanol to form a dispersion, wherein the solid-liquid mass ratio of the solid phase A dispersed in the ethanol to form a dispersion is solid / liquid = 1:30; stirring the dispersion, and then adding aluminum isopropoxide to the dispersion under stirring, wherein the mass ratio of the aluminum isopropoxide added to the dispersion to the mass ratio of the solid phase A in the dispersion is aluminum isopropoxide: solid phase A = 5:1; after the addition is completed, stirring and isothermal heating is performed in a water bath at 50±3°C for 3 hours. The dispersion was stirred for 50 minutes, and then the dispersion was spread in a glass dish and dried at 85°C to remove ethanol; the dried solid phase was calcined at 500°C for 1 hour in an argon atmosphere, and then cooled to room temperature in an argon atmosphere to obtain an aluminum oxide-coated powder; the aluminum oxide-coated powder was immersed in the aqueous solution of lithium hydroxide for 5 minutes, and the solid-liquid mass ratio of the aluminum oxide-coated powder immersed in the aqueous solution of lithium hydroxide was solid / liquid = 1:80; then the solid and liquid were separated, and the solid phase was calcined at 500°C for 1 hour again to obtain a solid phase B;

[0022] (3) A mixed solution of the solid phase B, pentafluoropyridine, ethylene glycol, ethanol and deionized water is prepared in a reaction kettle, wherein the mass ratio of the mixed solution of the solid phase B, pentafluoropyridine, ethylene glycol, ethanol and deionized water is solid phase B: pentafluoropyridine: ethylene glycol: ethanol: deionized water = 1:0.4:3:50:16; an ethanol solution of tetrabutyl titanate is prepared, wherein the mass percentage of tetrabutyl titanate in the ethanol solution of tetrabutyl titanate is 20%; the mixed solution is stirred, and the ethanol solution of tetrabutyl titanate is added to the mixed solution under stirring, wherein the mass ratio of the ethanol solution of tetrabutyl titanate added to the mixed solution to the mass ratio of the solid phase B in the mixed solution is tetrabutyl titanate ethanol solution: solid phase B = 20:1; after the addition is completed, the reaction kettle is closed, heated to 110° C. and kept warm for 8 hours, and then air-cooled to room temperature, the reaction kettle is opened, the solid-liquid separation is carried out, the solid phase is washed 3 times with ethanol, and then washed 3 times with deionized water, and dried to obtain the modified oxide powder.

[0023] The method for preparing the interior wall ceramic tile comprises the following steps:

[0024] Step 1, weighing each raw material component according to the weight proportion, mixing the raw materials, adding water to wet ball milling to obtain a slurry; the wet ball milling process is: the mass ratio of material, ball, and water is material: ball: water = 1:1.5:1; the ball milling speed is 120r / min, and the ball milling time is 8h;

[0025] Step 2: The slurry is sprayed and granulated to obtain powder, and the water content of the powder is adjusted to 5wt%; the powder is pressed into shape and fired, and the pressing and molding pressure is 60MPa; the firing temperature is 1200°C, and the firing time is 2h. After the firing is completed, the ceramic bricks are cooled to room temperature with the furnace; the interior wall ceramic tiles are obtained.

[0026] Example 2

[0027] A high-strength interior wall ceramic tile, comprising raw materials: clay, potassium feldspar powder, modified oxide powder, boron trioxide, zirconium oxide, yttrium oxide, titanium carbide, quartz powder, hydroxy calcium phosphate powder and barium carbonate; the raw material components are calculated by weight as follows: 50 parts of clay, 24 parts of potassium feldspar powder, 12 parts of modified oxide powder, 9 parts of boron trioxide, 4 parts of zirconium oxide, 4 parts of yttrium oxide, 7 parts of titanium carbide, 12 parts of quartz powder, 4 parts of hydroxy calcium phosphate powder and 2 parts of barium carbonate; each raw material component is a sieved powder passing through a 300-mesh sieve; the preparation method of the modified oxide powder is as follows:

[0028] (1) A zinc nitrate aqueous solution is prepared in a reaction kettle, wherein the concentration of zinc nitrate in the zinc nitrate aqueous solution is 0.03 mol / L, and the solvent is water; the zinc nitrate aqueous solution is stirred, and then hexamethylenetetramine is added to the solution under stirring, and the mass ratio of hexamethylenetetramine added to the solution is hexamethylenetetramine: solution = 4 g: 1 L; after the addition is completed, the solution is stirred for 10 minutes, and then ammonium dihydrogen phosphate is added to the solution under stirring, and the amount ratio of ammonium dihydrogen phosphate added to the solution is ammonium dihydrogen phosphate: solution = 8 g: 1 L; after the addition is completed, a sodium hydroxide solution is added, wherein the mass percentage of sodium hydroxide in the sodium hydroxide solution is 10%, and the solvent is water; the ratio of the added volume of the sodium hydroxide solution to the volume of the solution added thereto is sodium hydroxide solution: solution = 3:10; then the reaction kettle is closed, heated to 120±3° C., kept warm for 30 minutes, and then air-cooled to room temperature, the reaction kettle is opened, the solid-liquid separation is carried out, the solid phase is washed 3 times with deionized water, and dried to obtain a solid phase A;

[0029] (2) preparing an aqueous solution of lithium hydroxide; in the aqueous solution of lithium hydroxide, the concentration of lithium hydroxide is 20 g / L, and the solvent is water; dispersing the solid phase A in ethanol to form a dispersion, wherein the solid-liquid mass ratio of the solid phase A dispersed in the ethanol to form a dispersion is solid / liquid = 1:30; stirring the dispersion, and then adding aluminum isopropoxide to the dispersion under stirring, wherein the mass ratio of the aluminum isopropoxide added to the dispersion to the mass ratio of the solid phase A in the dispersion is aluminum isopropoxide: solid phase A = 6:1; after the addition is completed, stirring and isothermal heating in a water bath at 50±3°C for 3 hours; The dispersion was stirred for 50 minutes, and then the dispersion was spread in a glass dish and dried at 85°C to remove ethanol; the dried solid phase was calcined at 500°C for 1 hour in an argon atmosphere, and then cooled to room temperature in an argon atmosphere to obtain an aluminum oxide-coated powder; the aluminum oxide-coated powder was immersed in the aqueous solution of lithium hydroxide for 5 minutes, and the solid-liquid mass ratio of the aluminum oxide-coated powder immersed in the aqueous solution of lithium hydroxide was solid / liquid = 1:80; then the solid and liquid were separated, and the solid phase was calcined at 500°C for 1 hour again to obtain a solid phase B;

[0030] (3) A mixed solution of the solid phase B, pentafluoropyridine, ethylene glycol, ethanol and deionized water is prepared in a reaction kettle, wherein the mass ratio of the mixed solution of the solid phase B, pentafluoropyridine, ethylene glycol, ethanol and deionized water is solid phase B: pentafluoropyridine: ethylene glycol: ethanol: deionized water = 1:0.5:4:55:17; an ethanol solution of tetrabutyl titanate is prepared, wherein the mass percentage of tetrabutyl titanate in the ethanol solution of tetrabutyl titanate is 20%; the mixed solution is stirred, and the ethanol solution of tetrabutyl titanate is added to the mixed solution under stirring, and the mass ratio of the ethanol solution of tetrabutyl titanate added to the mixed solution to the mass ratio of the solid phase B in the mixed solution is tetrabutyl titanate ethanol solution: solid phase B = 20:1; after the addition is completed, the reaction kettle is closed, heated to 110° C. and kept warm for 8 hours, and then air-cooled to room temperature, the reaction kettle is opened, the solid-liquid separation is carried out, the solid phase is washed 3 times with ethanol, and then washed 3 times with deionized water, and dried to obtain the modified oxide powder.

[0031] The method for preparing the interior wall ceramic tile comprises the following steps:

[0032] Step 1, weighing each raw material component according to the weight proportion, mixing the raw materials, adding water to wet ball milling to obtain a slurry; the wet ball milling process is: the mass ratio of material, ball, and water is material: ball: water = 1:1.5:1; the ball milling speed is 120r / min, and the ball milling time is 8h;

[0033] Step 2: The slurry is sprayed and granulated to obtain powder, and the water content of the powder is adjusted to 5wt%; the powder is pressed into shape and fired, and the pressing and molding pressure is 60MPa; the firing temperature is 1200°C, and the firing time is 2h. After the firing is completed, the ceramic bricks are cooled to room temperature with the furnace; the interior wall ceramic tiles are obtained.

[0034] Example 3

[0035] A high-strength interior wall ceramic tile, comprising raw materials: clay, potassium feldspar powder, modified oxide powder, diboron trioxide, zirconium oxide, yttrium oxide, titanium carbide, quartz powder, hydroxy calcium phosphate powder and barium carbonate; the raw material components are calculated by weight as follows: 50 parts of clay, 27 parts of potassium feldspar powder, 14 parts of modified oxide powder, 9 parts of diboron trioxide, 4 parts of zirconium oxide, 4 parts of yttrium oxide, 7 parts of titanium carbide, 12 parts of quartz powder, 5 parts of hydroxy calcium phosphate powder and 3 parts of barium carbonate; each raw material component is a sieved powder passing through a 300-mesh sieve; the preparation method of the modified oxide powder is as follows:

[0036] (1) A zinc nitrate aqueous solution is prepared in a reactor, wherein the concentration of zinc nitrate in the zinc nitrate aqueous solution is 0.04 mol / L, and the solvent is water; the zinc nitrate aqueous solution is stirred, and then hexamethylenetetramine is added to the solution under stirring, and the mass ratio of hexamethylenetetramine added to the solution is hexamethylenetetramine: solution = 5 g: 1 L; after the addition is completed, the solution is stirred for 10 minutes, and then ammonium dihydrogen phosphate is added to the solution under stirring, and the amount ratio of ammonium dihydrogen phosphate added to the solution is ammonium dihydrogen phosphate: solution = 9 g: 1 L; after the addition is completed, a sodium hydroxide solution is added, wherein the mass percentage of sodium hydroxide in the sodium hydroxide solution is 10%, and the solvent is water; the ratio of the added volume of the sodium hydroxide solution to the volume of the solution added thereto is sodium hydroxide solution: solution = 3:10; then the reactor is closed, heated to 120±3° C., kept warm for 30 minutes, and then air-cooled to room temperature, the reactor is opened, the solid-liquid separation is carried out, the solid phase is washed 3 times with deionized water, and dried to obtain a solid phase A;

[0037] (2) preparing an aqueous solution of lithium hydroxide; in the aqueous solution of lithium hydroxide, the concentration of lithium hydroxide is 20 g / L, and the solvent is water; dispersing the solid phase A in ethanol to form a dispersion, wherein the solid-liquid mass ratio of the solid phase A dispersed in the ethanol to form a dispersion is solid / liquid = 1:30; stirring the dispersion, and then adding aluminum isopropoxide to the dispersion under stirring, wherein the mass ratio of the aluminum isopropoxide added to the dispersion to the mass ratio of the solid phase A in the dispersion is aluminum isopropoxide: solid phase A = 7:1; after the addition is completed, stirring and isothermal dispersing in a water bath at 50±3°C for 3 hours; The dispersion was stirred for 50 minutes, and then the dispersion was spread in a glass dish and dried at 85°C to remove ethanol; the dried solid phase was calcined at 500°C for 1 hour in an argon atmosphere, and then cooled to room temperature in an argon atmosphere to obtain an aluminum oxide-coated powder; the aluminum oxide-coated powder was immersed in the aqueous solution of lithium hydroxide for 5 minutes, and the solid-liquid mass ratio of the aluminum oxide-coated powder immersed in the aqueous solution of lithium hydroxide was solid / liquid = 1:80; then the solid and liquid were separated, and the solid phase was calcined at 500°C for 1 hour again to obtain a solid phase B;

[0038] (3) A mixed solution of the solid phase B, pentafluoropyridine, ethylene glycol, ethanol and deionized water is prepared in a reaction kettle, wherein the mass ratio of the mixed solution of the solid phase B, pentafluoropyridine, ethylene glycol, ethanol and deionized water is solid phase B: pentafluoropyridine: ethylene glycol: ethanol: deionized water = 1:0.5:4:55:17; an ethanol solution of tetrabutyl titanate is prepared, wherein the mass percentage of tetrabutyl titanate in the ethanol solution of tetrabutyl titanate is 20%; the mixed solution is stirred, and the ethanol solution of tetrabutyl titanate is added to the mixed solution under stirring, and the mass ratio of the ethanol solution of tetrabutyl titanate added to the mixed solution to the mass ratio of the solid phase B in the mixed solution is tetrabutyl titanate ethanol solution: solid phase B = 20:1; after the addition is completed, the reaction kettle is closed, heated to 110° C. and kept warm for 8 hours, and then air-cooled to room temperature, the reaction kettle is opened, the solid-liquid separation is carried out, the solid phase is washed 3 times with ethanol, and then washed 3 times with deionized water, and dried to obtain the modified oxide powder.

[0039] The method for preparing the interior wall ceramic tile comprises the following steps:

[0040] Step 1, weighing each raw material component according to the weight proportion, mixing the raw materials, adding water to wet ball milling to obtain a slurry; the wet ball milling process is: the mass ratio of material, ball, and water is material: ball: water = 1:1.5:1; the ball milling speed is 120r / min, and the ball milling time is 8h;

[0041] Step 2: The slurry is sprayed and granulated to obtain powder, and the water content of the powder is adjusted to 5wt%; the powder is pressed into shape and fired, and the pressing and molding pressure is 60MPa; the firing temperature is 1200°C, and the firing time is 2h. After the firing is completed, the ceramic bricks are cooled to room temperature with the furnace; the interior wall ceramic tiles are obtained.

[0042] Example 4

[0043] A high-strength interior wall ceramic tile, comprising raw materials: clay, potassium feldspar powder, modified oxide powder, diboron trioxide, zirconium oxide, yttrium oxide, titanium carbide, quartz powder, hydroxy calcium phosphate powder and barium carbonate; the raw material components are calculated by weight as follows: 50 parts of clay, 30 parts of potassium feldspar powder, 16 parts of modified oxide powder, 10 parts of diboron trioxide, 5 parts of zirconium oxide, 5 parts of yttrium oxide, 9 parts of titanium carbide, 14 parts of quartz powder, 6 parts of hydroxy calcium phosphate powder and 3 parts of barium carbonate; each raw material component is a sieved powder passing through a 300-mesh sieve; the preparation method of the modified oxide powder is as follows:

[0044] (1) A zinc nitrate aqueous solution is prepared in a reaction kettle, wherein the concentration of zinc nitrate in the zinc nitrate aqueous solution is 0.04 mol / L, and the solvent is water; the zinc nitrate aqueous solution is stirred, and then hexamethylenetetramine is added to the solution under stirring, and the mass ratio of hexamethylenetetramine added to the solution is hexamethylenetetramine: solution = 5 g: 1 L; after the addition is completed, the solution is stirred for 10 minutes, and then ammonium dihydrogen phosphate is added to the solution under stirring, and the amount ratio of ammonium dihydrogen phosphate added to the solution is ammonium dihydrogen phosphate: solution = 10 g: 1 L; after the addition is completed, a sodium hydroxide solution is added, wherein the mass percentage of sodium hydroxide in the sodium hydroxide solution is 10%, and the solvent is water; the ratio of the added volume of the sodium hydroxide solution to the volume of the solution added thereto is sodium hydroxide solution: solution = 4:10; then the reaction kettle is closed, heated to 120±3° C., kept warm for 30 minutes, and then air-cooled to room temperature, the reaction kettle is opened, the solid-liquid separation is carried out, the solid phase is washed 3 times with deionized water, and dried to obtain a solid phase A;

[0045] (2) preparing an aqueous solution of lithium hydroxide; in the aqueous solution of lithium hydroxide, the concentration of lithium hydroxide is 20 g / L, and the solvent is water; dispersing the solid phase A in ethanol to form a dispersion, wherein the solid-liquid mass ratio of the solid phase A dispersed in the ethanol to form a dispersion is solid / liquid = 1:30; stirring the dispersion, and then adding aluminum isopropoxide to the dispersion under stirring, wherein the mass ratio of the aluminum isopropoxide added to the dispersion to the mass ratio of the solid phase A in the dispersion is aluminum isopropoxide: solid phase A = 8:1; after the addition is completed, stirring and isothermal dispersing in a water bath at 50±3°C for 3 hours; The dispersion was stirred for 50 minutes, and then the dispersion was spread in a glass dish and dried at 85°C to remove ethanol; the dried solid phase was calcined at 500°C for 1 hour in an argon atmosphere, and then cooled to room temperature in an argon atmosphere to obtain an aluminum oxide-coated powder; the aluminum oxide-coated powder was immersed in the aqueous solution of lithium hydroxide for 5 minutes, and the solid-liquid mass ratio of the aluminum oxide-coated powder immersed in the aqueous solution of lithium hydroxide was solid / liquid = 1:80; then the solid and liquid were separated, and the solid phase was calcined at 500°C for 1 hour again to obtain a solid phase B;

[0046] (3) A mixed solution of the solid phase B, pentafluoropyridine, ethylene glycol, ethanol and deionized water is prepared in a reaction kettle, wherein the mass ratio of the solid phase B, pentafluoropyridine, ethylene glycol, ethanol and deionized water is solid phase B: pentafluoropyridine: ethylene glycol: ethanol: deionized water = 1:0.6:5:60:18; an ethanol solution of tetrabutyl titanate is prepared, wherein the mass percentage of tetrabutyl titanate in the ethanol solution of tetrabutyl titanate is 20%; the mixed solution is stirred, and the ethanol solution of tetrabutyl titanate is added to the mixed solution under stirring, wherein the mass ratio of the ethanol solution of tetrabutyl titanate added to the mixed solution to the mass ratio of the solid phase B in the mixed solution is tetrabutyl titanate: solid phase B = 20:1; after the addition is completed, the reaction kettle is closed, heated to 110° C. and kept warm for 8 hours, and then air-cooled to room temperature, the reaction kettle is opened, the solid-liquid separation is carried out, the solid phase is washed 3 times with ethanol, and then washed 3 times with deionized water, and dried to obtain the modified oxide powder.

[0047] The method for preparing the interior wall ceramic tile comprises the following steps:

[0048] Step 1, weighing each raw material component according to the weight proportion, mixing the raw materials, adding water to wet ball milling to obtain a slurry; the wet ball milling process is: the mass ratio of material, ball, and water is material: ball: water = 1:1.5:1; the ball milling speed is 120r / min, and the ball milling time is 8h;

[0049] Step 2: The slurry is sprayed and granulated to obtain powder, and the water content of the powder is adjusted to 5wt%; the powder is pressed into shape and fired, and the pressing and molding pressure is 60MPa; the firing temperature is 1200°C, and the firing time is 2h. After the firing is completed, the ceramic bricks are cooled to room temperature with the furnace; the interior wall ceramic tiles are obtained.

[0050] Comparative Example 1

[0051] A comparative interior wall ceramic tile, the raw materials include: clay, potassium feldspar powder, modified oxide powder, diboron trioxide, zirconium oxide, yttrium oxide, titanium carbide, quartz powder, hydroxy calcium phosphate powder and barium carbonate; the raw material components are calculated by weight: 50 parts of clay, 27 parts of potassium feldspar powder, 14 parts of modified oxide powder, 9 parts of diboron trioxide, 4 parts of zirconium oxide, 4 parts of yttrium oxide, 7 parts of titanium carbide, 12 parts of quartz powder, 5 parts of hydroxy calcium phosphate powder, 3 parts of barium carbonate; each raw material component is a sieved powder passing through a 300-mesh sieve; the preparation method of the modified oxide powder is:

[0052] (1) preparing an aqueous solution of zinc nitrate in a reactor, wherein the concentration of zinc nitrate in the aqueous solution is 0.04 mol / L, and the solvent is water; stirring the aqueous solution of zinc nitrate, and then adding hexamethylenetetramine to the solution under stirring, wherein the mass ratio of hexamethylenetetramine added to the solution is hexamethylenetetramine:solution=5 g:1 L; stirring the solution for 10 min after the addition is completed, and then adding a sodium hydroxide solution, wherein the mass percentage of sodium hydroxide in the sodium hydroxide solution is 10%, and the solvent is water; the ratio of the added volume of the sodium hydroxide solution to the volume of the solution added thereto is sodium hydroxide solution:solution=3:10; then closing the reactor, heating to 120±3° C., keeping the temperature for 30 min, and then air cooling to room temperature, opening the reactor, separating the solid from the liquid, washing the solid phase with deionized water for 3 times, and drying to obtain a solid phase A;

[0053] (2) preparing an aqueous solution of lithium hydroxide; in the aqueous solution of lithium hydroxide, the concentration of lithium hydroxide is 20 g / L, and the solvent is water; dispersing the solid phase A in ethanol to form a dispersion, wherein the solid-liquid mass ratio of the solid phase A dispersed in the ethanol to form a dispersion is solid / liquid = 1:30; stirring the dispersion, and then adding aluminum isopropoxide to the dispersion under stirring, wherein the mass ratio of the aluminum isopropoxide added to the dispersion to the mass ratio of the solid phase A in the dispersion is aluminum isopropoxide: solid phase A = 7:1; after the addition is completed, stirring and isothermal dispersing in a water bath at 50±3°C for 3 hours; The dispersion was stirred for 50 minutes, and then the dispersion was spread in a glass dish and dried at 85°C to remove ethanol; the dried solid phase was calcined at 500°C for 1 hour in an argon atmosphere, and then cooled to room temperature in an argon atmosphere to obtain an aluminum oxide-coated powder; the aluminum oxide-coated powder was immersed in the aqueous solution of lithium hydroxide for 5 minutes, and the solid-liquid mass ratio of the aluminum oxide-coated powder immersed in the aqueous solution of lithium hydroxide was solid / liquid = 1:80; then the solid and liquid were separated, and the solid phase was calcined at 500°C for 1 hour again to obtain a solid phase B;

[0054] (3) A mixed solution of the solid phase B, pentafluoropyridine, ethylene glycol, ethanol and deionized water is prepared in a reaction kettle, wherein the mass ratio of the mixed solution of the solid phase B, pentafluoropyridine, ethylene glycol, ethanol and deionized water is solid phase B: pentafluoropyridine: ethylene glycol: ethanol: deionized water = 1:0.5:4:55:17; an ethanol solution of tetrabutyl titanate is prepared, wherein the mass percentage of tetrabutyl titanate in the ethanol solution of tetrabutyl titanate is 20%; the mixed solution is stirred, and the ethanol solution of tetrabutyl titanate is added to the mixed solution under stirring, and the mass ratio of the ethanol solution of tetrabutyl titanate added to the mixed solution to the mass ratio of the solid phase B in the mixed solution is tetrabutyl titanate ethanol solution: solid phase B = 20:1; after the addition is completed, the reaction kettle is closed, heated to 110° C. and kept warm for 8 hours, and then air-cooled to room temperature, the reaction kettle is opened, the solid-liquid separation is carried out, the solid phase is washed 3 times with ethanol, and then washed 3 times with deionized water, and dried to obtain the modified oxide powder.

[0055] The method for preparing the interior wall ceramic tile comprises the following steps:

[0056] Step 1, weighing each raw material component according to the weight proportion, mixing the raw materials, adding water to wet ball milling to obtain a slurry; the wet ball milling process is: the mass ratio of material, ball, and water is material: ball: water = 1:1.5:1; the ball milling speed is 120r / min, and the ball milling time is 8h;

[0057] Step 2: The slurry is sprayed and granulated to obtain powder, and the water content of the powder is adjusted to 5wt%; the powder is pressed into shape and fired, and the pressing and molding pressure is 60MPa; the firing temperature is 1200°C, and the firing time is 2h. After the firing is completed, the ceramic brick is cooled to room temperature with the furnace; the interior wall ceramic brick described in this comparative example is obtained.

[0058] Comparative Example 2

[0059] A comparative interior wall ceramic tile, the raw materials include: clay, potassium feldspar powder, modified oxide powder, diboron trioxide, zirconium oxide, yttrium oxide, titanium carbide, quartz powder, hydroxy calcium phosphate powder and barium carbonate; the raw material components are calculated by weight: 50 parts of clay, 27 parts of potassium feldspar powder, 14 parts of modified oxide powder, 9 parts of diboron trioxide, 4 parts of zirconium oxide, 4 parts of yttrium oxide, 7 parts of titanium carbide, 12 parts of quartz powder, 5 parts of hydroxy calcium phosphate powder, 3 parts of barium carbonate; each raw material component is a sieved powder passing through a 300-mesh sieve; the preparation method of the modified oxide powder is:

[0060] (1) A zinc nitrate aqueous solution is prepared in a reactor, wherein the concentration of zinc nitrate in the zinc nitrate aqueous solution is 0.04 mol / L, and the solvent is water; the zinc nitrate aqueous solution is stirred, and then hexamethylenetetramine is added to the solution under stirring, and the mass ratio of hexamethylenetetramine added to the solution is hexamethylenetetramine: solution = 5 g: 1 L; after the addition is completed, the solution is stirred for 10 minutes, and then ammonium dihydrogen phosphate is added to the solution under stirring, and the amount ratio of ammonium dihydrogen phosphate added to the solution is ammonium dihydrogen phosphate: solution = 9 g: 1 L; after the addition is completed, a sodium hydroxide solution is added, wherein the mass percentage of sodium hydroxide in the sodium hydroxide solution is 10%, and the solvent is water; the ratio of the added volume of the sodium hydroxide solution to the volume of the solution added thereto is sodium hydroxide solution: solution = 3:10; then the reactor is closed, heated to 120±3° C., kept warm for 30 minutes, and then air-cooled to room temperature, the reactor is opened, the solid-liquid separation is carried out, the solid phase is washed 3 times with deionized water, and dried to obtain a solid phase A;

[0061] (2) A mixture of the solid phase A, pentafluoropyridine, ethylene glycol, ethanol and deionized water is prepared in a reactor, wherein the mass ratio of the solid phase A, pentafluoropyridine, ethylene glycol, ethanol and deionized water is solid phase A: pentafluoropyridine: ethylene glycol: ethanol: deionized water = 1:0.5:4:55:17; an ethanol solution of tetrabutyl titanate is prepared, wherein the mass percentage of tetrabutyl titanate in the ethanol solution of tetrabutyl titanate is 20%; the mixed solution is stirred, and the ethanol solution of tetrabutyl titanate is added to the mixed solution under stirring, and the mass ratio of the ethanol solution of tetrabutyl titanate added to the mixed solution to the mass ratio of the solid phase A in the mixed solution is tetrabutyl titanate ethanol solution: solid phase A = 20:1; after the addition is completed, the reactor is closed, heated to 110° C. and kept warm for 8 hours, and then air-cooled to room temperature, the reactor is opened, the solid-liquid separation is carried out, the solid phase is washed 3 times with ethanol, and then washed 3 times with deionized water, and dried to obtain the modified oxide powder.

[0062] The method for preparing the interior wall ceramic tile comprises the following steps:

[0063] Step 1, weighing each raw material component according to the weight proportion, mixing the raw materials, adding water to wet ball milling to obtain a slurry; the wet ball milling process is: the mass ratio of material, ball, and water is material: ball: water = 1:1.5:1; the ball milling speed is 120r / min, and the ball milling time is 8h;

[0064] Step 2: The slurry is sprayed and granulated to obtain powder, and the water content of the powder is adjusted to 5wt%; the powder is pressed into shape and fired, and the pressing and molding pressure is 60MPa; the firing temperature is 1200°C, and the firing time is 2h. After the firing is completed, the ceramic brick is cooled to room temperature with the furnace; the interior wall ceramic brick described in this comparative example is obtained.

[0065] Comparative Example 3

[0066] A comparative interior wall ceramic tile, the raw materials include: clay, potassium feldspar powder, modified oxide powder, diboron trioxide, zirconium oxide, yttrium oxide, titanium carbide, quartz powder, hydroxy calcium phosphate powder and barium carbonate; the raw material components are calculated by weight: 50 parts of clay, 27 parts of potassium feldspar powder, 14 parts of modified oxide powder, 9 parts of diboron trioxide, 4 parts of zirconium oxide, 4 parts of yttrium oxide, 7 parts of titanium carbide, 12 parts of quartz powder, 5 parts of hydroxy calcium phosphate powder, 3 parts of barium carbonate; each raw material component is a sieved powder passing through a 300-mesh sieve; the preparation method of the modified oxide powder is:

[0067] (1) A zinc nitrate aqueous solution is prepared in a reactor, wherein the concentration of zinc nitrate in the zinc nitrate aqueous solution is 0.04 mol / L, and the solvent is water; the zinc nitrate aqueous solution is stirred, and then hexamethylenetetramine is added to the solution under stirring, and the mass ratio of hexamethylenetetramine added to the solution is hexamethylenetetramine: solution = 5 g: 1 L; after the addition is completed, the solution is stirred for 10 minutes, and then ammonium dihydrogen phosphate is added to the solution under stirring, and the amount ratio of ammonium dihydrogen phosphate added to the solution is ammonium dihydrogen phosphate: solution = 9 g: 1 L; after the addition is completed, a sodium hydroxide solution is added, wherein the mass percentage of sodium hydroxide in the sodium hydroxide solution is 10%, and the solvent is water; the ratio of the added volume of the sodium hydroxide solution to the volume of the solution added thereto is sodium hydroxide solution: solution = 3:10; then the reactor is closed, heated to 120±3° C., kept warm for 30 minutes, and then air-cooled to room temperature, the reactor is opened, the solid-liquid separation is carried out, the solid phase is washed 3 times with deionized water, and dried to obtain a solid phase A;

[0068] (2) preparing an aqueous solution of lithium hydroxide; in the aqueous solution of lithium hydroxide, the concentration of lithium hydroxide is 20 g / L, and the solvent is water; dispersing the solid phase A in ethanol to form a dispersion, wherein the solid-liquid mass ratio of the solid phase A dispersed in the ethanol to form a dispersion is solid / liquid = 1:30; stirring the dispersion, and then adding aluminum isopropoxide to the dispersion under stirring, wherein the mass ratio of the aluminum isopropoxide added to the dispersion to the mass ratio of the solid phase A in the dispersion is aluminum isopropoxide: solid phase A = 7:1; after the addition is completed, stirring the dispersion in a water bath at a constant temperature of 50±3°C for 50 min. in, and then spread the dispersion in a glass dish and dry it at 85°C to remove ethanol; the dried solid phase is calcined at 500°C in an argon atmosphere for 1 hour, and then cooled to room temperature in an argon atmosphere to obtain an aluminum oxide-coated powder; the aluminum oxide-coated powder is immersed in the aqueous solution of lithium hydroxide for 5 minutes, and the solid-liquid mass ratio of the aluminum oxide-coated powder immersed in the aqueous solution of lithium hydroxide is solid / liquid=1:80; then the solid and liquid are separated, and the solid phase is calcined at 500°C again for 1 hour to obtain the modified oxide powder described in this comparative example.

[0069] The method for preparing the interior wall ceramic tile comprises the following steps:

[0070] Step 1, weighing each raw material component according to the weight proportion, mixing the raw materials, adding water to wet ball milling to obtain a slurry; the wet ball milling process is: the mass ratio of material, ball, and water is material: ball: water = 1:1.5:1; the ball milling speed is 120r / min, and the ball milling time is 8h;

[0071] Step 2: The slurry is sprayed and granulated to obtain powder, and the water content of the powder is adjusted to 5wt%; the powder is pressed into shape and fired, and the pressing and molding pressure is 60MPa; the firing temperature is 1200°C, and the firing time is 2h. After the firing is completed, the ceramic brick is cooled to room temperature with the furnace; the interior wall ceramic brick described in this comparative example is obtained.

[0072] Example 5

[0073] According to the requirements of standard GB / T2542-2012, the bending strength and water absorption rate of the interior wall ceramic tiles obtained in the above embodiments and comparative examples were tested respectively, as shown in Table 1.

[0074] Table 1

[0075] Experimental Group Bending strength / MPa Water absorption / % Example 1 71.3 9.5 Example 2 73.6 9.1 Example 3 74.2 8.8 Example 4 73.9 9.0 Comparative Example 1 62.0 15.3 Comparative Example 2 50.7 13.6 Comparative Example 3 52.8 12.4

[0076] As shown in Table 1, the interior wall ceramic tile prepared by the method of the present invention has high bending strength, excellent mechanical properties, low water absorption, dense structure, fewer defects and holes, and significantly improves the durability of the ceramic tile. By comparing Example 3 and each comparative example, it can be seen that the addition of the modified oxide powder in the present invention can significantly improve the strength of the ceramic and improve the density. This is mainly because on the one hand, a coating layer that is easy to compound with components such as boron oxide and clay is formed on the surface of the modified oxide powder, thereby increasing the bonding strength between the components. On the other hand, a low eutectic is formed on the surface of the modified oxide powder during the firing process, and the pores and defects between the two phase interfaces are filled by the low eutectic with a certain fluidity, thereby improving the overall density of the material.

[0077] The technical solution provided by the present invention is introduced in detail above. For those skilled in the art, according to the concept of the embodiments of the present invention, there may be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A high-strength interior wall ceramic tile, characterized in that: The raw materials include: clay, potassium feldspar powder, modified oxide powder, boron trioxide, zirconium oxide, yttrium oxide, titanium carbide, quartz powder, hydroxy calcium phosphate powder and barium carbonate; the raw material components are calculated by weight as follows: 50 parts of clay, 20-30 parts of potassium feldspar powder, 10-16 parts of modified oxide powder, 8-10 parts of boron trioxide, 3-5 parts of zirconium oxide, 3-5 parts of yttrium oxide, 4-9 parts of titanium carbide, 10-14 parts of quartz powder, 3-6 parts of hydroxy calcium phosphate powder, and 2-3 parts of barium carbonate; all raw material components are sieved powders passing through a 300-mesh sieve; the preparation method of the modified oxide powder is: (1) A zinc nitrate aqueous solution is prepared in a reactor, wherein the concentration of zinc nitrate in the zinc nitrate aqueous solution is 0.03-0.04 mol / L, and the solvent is water; the zinc nitrate aqueous solution is stirred, and then hexamethylenetetramine is added to the solution under stirring, and the mass ratio of hexamethylenetetramine added to the solution is hexamethylenetetramine: solution = 4-5 g: 1 L; after the addition is completed, the solution is stirred for more than 10 minutes, and then ammonium dihydrogen phosphate is added to the solution under stirring, and the amount ratio of ammonium dihydrogen phosphate added to the solution is ammonium dihydrogen phosphate: solution = 7-10 g: 1 L; after the addition is completed, a sodium hydroxide solution is added, wherein the mass percentage of sodium hydroxide in the sodium hydroxide solution is 10%, and the solvent is water; the ratio of the added volume of the sodium hydroxide solution to the volume of the solution added thereto is sodium hydroxide solution: solution = 2-4:10; then the reactor is closed, heated to 120±3° C., kept warm for more than 30 minutes, and then air-cooled to room temperature, the reactor is opened, the solid-liquid separation is carried out, the solid phase is washed with deionized water, and dried to obtain a solid phase A; (2) preparing an aqueous solution of lithium hydroxide; in the aqueous solution of lithium hydroxide, the concentration of lithium hydroxide is 20 g / L, and the solvent is water; Dispersing in ethanol to form a dispersion, the solid phase A is dispersed in ethanol to form a dispersion with a solid / liquid mass ratio of 1:30; stirring the dispersion, and then adding aluminum isopropoxide to the dispersion under stirring, the mass ratio of aluminum isopropoxide added to the dispersion to the mass ratio of solid phase A in the dispersion is aluminum isopropoxide: solid phase A=5-8:1; after the addition is completed, the dispersion is stirred at a constant temperature of 50±3°C in a water bath for more than 50 minutes, and then the dispersion is spread in a glass dish, and dried at 85°C to remove ethanol; the dried solid phase is placed at 500°C for calcination for more than 1 hour in an argon atmosphere, and then cooled to room temperature in an argon atmosphere to obtain an aluminum oxide coated powder; soaking the aluminum oxide coated powder in the aqueous solution of lithium hydroxide for 4-5 minutes, and the solid-liquid mass ratio of the aluminum oxide coated powder soaked in the aqueous solution of lithium hydroxide is solid / liquid=1:80; then the solid and liquid are separated, and the solid phase is placed at 500°C for calcination for more than 1 hour again to obtain a solid phase B; (3) In a reaction kettle, a mixture of the solid phase B, pentafluoropyridine, ethylene glycol, ethanol and deionized water is prepared, wherein the mass ratio of the solid phase B, pentafluoropyridine, ethylene glycol, ethanol and deionized water is solid phase B: pentafluoropyridine: ethylene glycol: ethanol: deionized water = 1: 0.4-0.6: 3-5: 50-60: 16-18; an ethanol solution of tetrabutyl titanate is prepared; the mass percentage of tetrabutyl titanate in the ethanol solution of tetrabutyl titanate is 20%, and the mixture is stirred. In this state, the ethanol solution of tetrabutyl titanate is added to the mixed solution, and the mass ratio of the ethanol solution of tetrabutyl titanate added to the mixed solution to the mass ratio of the solid phase B in the mixed solution is the ethanol solution of tetrabutyl titanate: solid phase B = 20:1; after the addition is completed, the reactor is closed, heated to 110°C and kept warm for more than 8 hours, and then air-cooled to room temperature, the reactor is opened, the solid-liquid separation is carried out, the solid phase is washed with ethanol for more than 3 times, and then washed with deionized water for more than 3 times, and dried to obtain the modified oxide powder.

2. The method for preparing interior wall ceramic tiles according to claim 1, characterized in that the steps include: Step 1, weighing each raw material component according to the weight proportion, mixing the raw materials, adding water to wet-mill the mixture, and obtaining a slurry; Step 2: spray granulate the slurry to obtain powder, and adjust the water content of the powder to 5wt%; press the powder into shape, and fire it to obtain the interior wall ceramic tile.

3. A preparation method according to claim 2, characterized in that: The wet ball milling process is as follows: the mass ratio of material, ball and water is material: ball: water = 1:1.5:1; the ball milling speed is 120r / min, and the ball milling time is 8h; the pressing molding pressure is 60MPa; the firing temperature is 1200°C, and the firing time is 2h. After the firing is completed, the ceramic bricks are cooled to room temperature with the furnace.