Preparation method and application of Co-modified RuO2 material

Co-modified RuO2 materials were prepared by hydrothermal synthesis and oxidation, which solved the problem of high cost of precious metal catalysts and achieved efficient and stable ORR/OER performance. It is suitable as an anode catalyst for zinc-air batteries and has practical application value.

CN117577857BActive Publication Date: 2026-11-10HEILONGJIANG UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310328659.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2026-11-10
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

In existing zinc-air batteries, precious metal Pt and Ir-based catalysts are expensive and scarce, limiting their large-scale application. Furthermore, existing alternative catalysts perform poorly in the oxygen reduction reaction (ORR) and oxygen evolution reaction (OER).

Method used

Co-modified RuO2 materials were prepared by hydrothermal synthesis and oxidation methods and used as negative electrode catalysts for zinc-air batteries. This simple and easy-to-operate method reduces costs and improves ORR/OER catalytic activity and stability.

Benefits of technology

It achieves efficient and stable ORR/OER catalytic performance, can be assembled into zinc-air batteries to light LED lights, has practical application value, and can be used on a large scale.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117577857B_ABST
    Figure CN117577857B_ABST
Patent Text Reader

Abstract

This application relates to the field of electrocatalytic materials technology, and more specifically, to a method for preparing and applying a Co-modified RuO2 material. The preparation method includes the following steps: S1: Weigh 1-10g of glucose and 0.1-1g of urea and dissolve them in 5-30ml of aqueous solution, stir for 10-50min to obtain a mixed solution, add 0.005-0.03g of cobalt salt and 0.03-0.05g of ruthenium salt to the mixed solution, continue stirring for 1-3h until the solution is clear, obtain a preparation solution, transfer the preparation solution to a hydrothermal reactor, heat, and centrifuge to collect the synthesized precursor; S2: Weigh 0.1-0.5g of the synthesized precursor and place it in a muffle furnace, calcine at 300-600℃ for 2-12h to obtain the final sample. This material has advantages such as high activity, good stability, and can be used as a negative electrode catalyst in zinc-air batteries. Assembling a complete zinc-air battery can light LED lights, demonstrating practical application value and the potential for large-scale use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of electrocatalytic materials technology, and more specifically, to a method for preparing and applying a Co-modified RuO2 material. Background Technology

[0002] With the rapid development of the modern economy, humanity is facing a series of increasingly severe environmental and energy problems. Green renewable energy, represented by wind and solar power, will occupy a dominant position in the energy structure. However, green renewable energy is susceptible to natural conditions, exhibiting intermittency, volatility, and uncontrollability, which seriously hinders its large-scale utilization. Batteries, as a new type of energy storage and conversion technology, hold the promise of solving these problems. Currently, lithium-ion batteries, due to their mature battery technology and dominant position in rechargeable batteries, have been widely used in many fields such as medical devices, portable electronic products, electric / hybrid vehicles, and the military. However, the high production cost, unsatisfactory energy density, and potential toxicity of lithium-ion batteries hinder their further large-scale development.

[0003] Metal-air batteries have garnered widespread attention due to their high theoretical energy density, low production cost, and safety and environmental friendliness. Zinc-air batteries, as a type of metal-air battery, are receiving increasing attention in this field due to their high energy density, long electrochemical stability, low internal resistance, low operating conditions, and abundant resources. The oxygen evolution reaction (OER) and oxygen reduction reaction (ORR) are the two most important reactions for energy storage and conversion in zinc-air batteries; therefore, researching efficient and stable bifunctional electrocatalysts with excellent ORR / OER performance is of great significance. Pt and Ru / Ir are effective ORR / OER catalysts, but their high cost and resource scarcity limit their large-scale use. Current research has demonstrated that certain metal catalysts can effectively reduce the use of these precious metals or replace their applications, including transition metal sulfides, oxides, carbides, and nitrides. These have shown good ORR / OER activity and durability, and can be assembled into zinc-air batteries with practical application value. Summary of the Invention

[0004] This disclosure provides a method for preparing and applying Co-modified RuO2 materials. These materials exhibit high activity and good stability, making them suitable as negative electrode catalysts in zinc-air batteries. When assembled into complete zinc-air batteries, they can power LED lights, demonstrating practical application value and the potential for large-scale use.

[0005] In a first aspect, this disclosure provides a method for preparing a Co-modified RuO2 material, comprising the following steps:

[0006] S1: Weigh 1-10g of glucose and 0.1-1g of urea and dissolve them in 5-30ml of aqueous solution. Stir for 10-50min to obtain a mixed solution. Add 0.005-0.03g of cobalt salt and 0.03-0.05g of ruthenium salt to the mixed solution and continue stirring for 1-3h until the solution is clear to obtain the preparation solution. Transfer the preparation solution to a hydrothermal reactor, heat it, and then centrifuge to collect the synthesized precursor.

[0007] S2: Weigh 0.1-0.5g of the synthesized precursor and place it in a muffle furnace to calcine at 300-600℃ for 2-12h to obtain the final sample.

[0008] Co-modified RuO2 materials were prepared by hydrothermal synthesis and oxidation, a method that is simple, easy to operate, and low in cost. Co-modified RuO2 obtained through a one-pot hydrothermal-oxidation method exhibits high ORR / OER catalytic activity and excellent cycling stability.

[0009] Preferably, it includes the following steps:

[0010] S1: Weigh 0.1-0.8g of glucose and 0.1-1g of urea and dissolve them in 5-30ml of aqueous solution. Stir for 10-50min to obtain a mixed solution. Add 0.005-0.03g of cobalt salt and 0.03-0.05g of ruthenium salt to the mixed solution and continue stirring for 1-3h until the solution is clear to obtain the preparation solution. Transfer the preparation solution to a hydrothermal reactor, heat it, and then centrifuge to collect the synthesized precursor.

[0011] S2: Weigh 0.1-0.5g of the synthesized precursor and place it in a muffle furnace to calcine at 300-600℃ for 2-12h to obtain the final sample.

[0012] Preferably, the heating process in step S1 is as follows: the temperature is set to 100-160℃ and the reaction time is 5-10h.

[0013] Preferably, the cobalt salt in S1 is one or more of cobalt nitrate, cobalt chloride, cobalt antimonide, and cobalt selenide.

[0014] Preferably, the ruthenium salt in S1 is ruthenium dioxide.

[0015] Secondly, this disclosure provides an application of a Co-modified RuO2 material catalyst, which can be used as a negative electrode catalyst in a zinc-air battery.

[0016] The Co-modified RuO2 material catalyst in this application can be used as a negative electrode catalyst in zinc-air batteries. When assembled into a complete zinc-air battery, it can light up LED lights, which has practical application value and can be used on a large scale.

[0017] Preferably, the specific method of application includes the following steps:

[0018] (1) Weigh 5 mg-10 mg of the prepared catalyst or Pt / C (10 wt.%, Pt) and disperse it in a mixture of 100 μL-150 μL of ethanol and 5 wt.% Nafion, and sonicate for 1 h to obtain a uniform catalyst ink.

[0019] (2) Coat 5 μL-10 μL of the catalyst ink onto the GCE and dry it at room temperature to obtain the working electrode.

[0020] In summary, this application has the following beneficial effects:

[0021] 1. Since the Co-modified RuO2 material is prepared by hydrothermal synthesis and oxidation in this application, the method is simple, easy to operate, and low in cost;

[0022] 2. The Co-modified RuO2 obtained by the one-pot hydrothermal-oxidation method in this application exhibits high ORR / OER catalytic activity and excellent cycle stability;

[0023] 3. The Co-modified RuO2 material catalyst in this application can be used as the negative electrode catalyst of zinc-air batteries. When assembled into a complete zinc-air battery, it can light up LED lights, which has practical application value and can be used on a large scale.

[0024] It should be understood that the above general description and the following detailed description are exemplary and explanatory only, and do not limit the scope of protection of this disclosure. Attached Figure Description

[0025] 1. Figure 1 The scanning electron microscope image of the precursor;

[0026] 2. Figure 2 The image shows a scanning electron microscope image of the Co-RuO2 material obtained in Example 1.

[0027] 3. Figure 3 The image shows a scanning electron microscope image of the Co-RuO2 material obtained in Example 2.

[0028] 4. Figure 4 Transmission electron microscope image of the Co-RuO2 material obtained in Example 2;

[0029] 5. Figure 5 The ORR stability diagram of the Co-RuO2 material obtained in Example 2 is shown.

[0030] 6. Figure 6 The diagram shows the OER stability of the Co-RuO2 material obtained in Example 2.

[0031] 7. Figure 7 The image shows a scanning electron microscope image of the Co-RuO2 material obtained in Example 3.

[0032] 8. Figure 8 The image shows a scanning electron microscope image of the Co-RuO2 material obtained in Example 4.

[0033] 9. Figure 9 ORR cyclic voltammetry (CV) performance graphs of the Co-RuO2 materials obtained in Examples 1, 2, 3 and 4;

[0034] 10. Figure 10 The ORR linear sweep voltammetry (LSV) performance graphs of the Co-RuO2 materials obtained in Examples 1, 2, 3 and 4 are shown.

[0035] 11. Figure 11 The OER linear sweep voltammetry (LSV) performance graphs of the Co-RuO2 materials obtained in Examples 1, 2, 3 and 4 are shown.

[0036] 12. Figure 12 The specific capacity curve of the Co-RuO2 material obtained in Example 2 as the negative electrode of a zinc-air battery is shown.

[0037] 13. Figure 13 for Figure 11 The stability curve of the Co-RuO2 material obtained in Example 2 as the negative electrode of a zinc-air battery is shown. Detailed Implementation

[0038] The following detailed description of this application is provided in conjunction with the embodiments. It should be noted that: unless otherwise specified, the conditions in the following embodiments are performed under conventional conditions or conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following embodiments are all from commercially available sources.

[0039] Example

[0040] Example 1

[0041] A method for preparing Co-modified RuO2 material includes the following steps:

[0042] S1: Weigh 5g of glucose and 1g of urea and dissolve them in 10ml of aqueous solution. Stir for 30min. After dissolution, add 0.0056g of cobalt salt and 0.032g of ruthenium salt, and continue stirring for 1.5h. Transfer the mixed solution to a hydrothermal reactor, set the temperature to 140℃, and react for 8h. Then, collect the synthesized precursor by centrifugation and analyze it under a scanning electron microscope as follows: Figure 1 The precursor exhibits a spherical structure;

[0043] S2: 0.1 g of the precursor was weighed and placed in a muffle furnace and calcined at 300 °C for 8 h to obtain a dry black powder Co-RuO2-300.

[0044] The scanning electron microscope image of the Co-modified RuO2 material obtained by this implementation scheme is as follows: Figure 2 As shown in the scan image, after calcination, the precursor changed from a spherical shape to a sheet-like shape, and the surface area increased, indicating that temperature has a certain influence on its morphology.

[0045] Example 2

[0046] A method for preparing Co-modified RuO2 material includes the following steps:

[0047] S1: Weigh 5g of glucose and 1g of urea and dissolve them in 10ml of aqueous solution. Stir for 30min. After dissolution, add 0.0056g of cobalt salt and 0.032g of ruthenium salt, and continue stirring for 1.5h. Transfer the mixed solution to a hydrothermal reactor, set the temperature to 140℃, and react for 8h. Then, collect the synthesized precursor by centrifugation and analyze it under a scanning electron microscope as follows: Figure 1 The precursor exhibits a spherical structure;

[0048] S2: Weigh 0.1g of the synthesized precursor and place it in a muffle furnace and calcine at 400℃ for 8h to obtain a dry black powder Co-RuO2-400.

[0049] The scanning electron microscope image of the Co-modified RuO2 material obtained by this implementation scheme is as follows: Figure 3 As shown, the transmission electron microscope image is as follows: Figure 4 As shown, the sheet becomes thinner when the calcination temperature is 400°C, indicating that temperature has a certain influence on its morphology. Figure 5 The ORR stability curve of Co-RuO2-400 obtained by chronoamperometry is shown below. Figure 6 The OER stability curve shows that it has good stability.

[0050] Example 3

[0051] A method for preparing Co-modified RuO2 material includes the following steps:

[0052] S1: Weigh 5g of glucose and 1g of urea and dissolve them in 10ml of aqueous solution. Stir for 30min. After dissolution, add 0.0056g of cobalt salt and 0.032g of ruthenium salt, and continue stirring for 1.5h. Transfer the mixed solution to a hydrothermal reactor, set the temperature to 140℃, and react for 8h. Then, collect the synthesized precursor by centrifugation and analyze it under a scanning electron microscope as follows: Figure 1 The precursor exhibits a spherical structure;

[0053] S2: Weigh 0.1g of the synthesized precursor and place it in a muffle furnace. Calcine it at 500℃ for 8h to obtain a dry black powder, Co-RuO2-500.

[0054] The scanning electron microscope image of the Co-modified RuO2 material obtained by this implementation scheme is as follows: Figure 7 As shown, the calcination temperature is 500°C, which indicates that the lamellae are too thin, suggesting that temperature has a certain influence on the control of their morphology. When the temperature is too high, the lamellae structure is easily damaged.

[0055] Example 4

[0056] A method for preparing Co-modified RuO2 material includes the following steps:

[0057] S1: Weigh 5g of glucose and 1g of urea and dissolve them in 10ml of aqueous solution. Stir for 30min. After dissolution, add 0.0056g of cobalt salt and 0.032g of ruthenium salt, and continue stirring for 1.5h. Transfer the mixed solution to a hydrothermal reactor, set the temperature to 140℃, and react for 8h. Then, collect the synthesized precursor by centrifugation and analyze it under a scanning electron microscope as follows: Figure 1 The precursor exhibits a spherical structure;

[0058] S2: Weigh 0.1 g of the synthesized precursor and place it in a muffle furnace and calcine at 600 °C for 8 h to obtain a dry black powder Co-RuO2-600.

[0059] The scanning electron microscope image of the Co-modified RuO2 material obtained by this implementation scheme is as follows: Figure 8 As shown.

[0060] Example 5

[0061] A method for preparing Co-modified RuO2 material includes the following steps:

[0062] S1: Weigh 0.5g glucose and 0.1g urea and dissolve them in 10ml of aqueous solution. Stir for 30min. After dissolution, add 0.0056g cobalt salt and 0.032g ruthenium salt, and continue stirring for 1.5h. Transfer the mixed solution to a hydrothermal reactor, set the temperature to 140℃, and react for 8h. Then, collect the synthesized precursor by centrifugation and analyze it under a scanning electron microscope as follows: Figure 1 The precursor exhibits a spherical structure;

[0063] S2: 0.1 g of the precursor was weighed and placed in a muffle furnace and calcined at 300 °C for 8 h to obtain a dry black powder Co-RuO2-300.

[0064] Example 6

[0065] A method for preparing Co-modified RuO2 material includes the following steps:

[0066] S1: Weigh 0.5g glucose and 0.1g urea and dissolve them in 10ml of aqueous solution. Stir for 30min. After dissolution, add 0.0056g cobalt salt and 0.032g ruthenium salt, and continue stirring for 1.5h. Transfer the mixed solution to a hydrothermal reactor, set the temperature to 140℃, and react for 8h. Then, collect the synthesized precursor by centrifugation and analyze it under a scanning electron microscope as follows: Figure 1 The precursor exhibits a spherical structure;

[0067] S2: Weigh 0.1g of the synthesized precursor and place it in a muffle furnace and calcine at 400℃ for 8h to obtain a dry black powder Co-RuO2-400.

[0068] Example 7

[0069] A method for preparing Co-modified RuO2 material includes the following steps:

[0070] S1: Weigh 0.5g glucose and 0.1g urea and dissolve them in 10ml of aqueous solution. Stir for 30min. After dissolution, add 0.0056g cobalt salt and 0.032g ruthenium salt, and continue stirring for 1.5h. Transfer the mixed solution to a hydrothermal reactor, set the temperature to 140℃, and react for 8h. Then, collect the synthesized precursor by centrifugation and analyze it under a scanning electron microscope as follows: Figure 1 The precursor exhibits a spherical structure;

[0071] S2: Weigh 0.1g of the synthesized precursor and place it in a muffle furnace. Calcine it at 500℃ for 8h to obtain a dry black powder, Co-RuO2-500.

[0072] Example 8

[0073] A method for preparing Co-modified RuO2 material includes the following steps:

[0074] S1: Weigh 0.5g glucose and 0.1g urea and dissolve them in 10ml of aqueous solution. Stir for 30min. After dissolution, add 0.0056g cobalt salt and 0.032g ruthenium salt, and continue stirring for 1.5h. Transfer the mixed solution to a hydrothermal reactor, set the temperature to 140℃, and react for 8h. Then, collect the synthesized precursor by centrifugation and analyze it under a scanning electron microscope as follows: Figure 1 The precursor exhibits a spherical structure;

[0075] S2: Weigh 0.1 g of the synthesized precursor and place it in a muffle furnace and calcine at 600 °C for 8 h to obtain a dry black powder Co-RuO2-600.

[0076] Comparative Example

[0077] Comparative Example 1

[0078] Co-modified RuO2 materials were prepared according to the method in Example 2, except that the temperature in S2 was below 300°C.

[0079] Comparative Example 2

[0080] Co-modified RuO2 materials were prepared according to the method in Example 2, except that glucose and urea were not added in S1.

[0081] Comparative Example 3

[0082] Co-modified RuO2 materials were prepared according to the method in Example 2, except that hydrothermal autoclave heating was not performed in S1.

[0083] Application examples

[0084] Application Example 1

[0085] An application of a Co-modified RuO2 catalyst was described, with electrochemical testing conducted in a 0.1 M KOH aqueous solution electrolyte using an electrochemical workstation (CHI1760E, Shanghai) with a typical three-electrode system. A Pt wire electrode and a saturated calomel electrode served as the counter and reference electrodes, respectively. A rotating disk electrode (RDE) with a 4.0 mm diameter glassy carbon electrode (GCE) was used as the working substrate electrode.

[0086] (1) Weigh 5 mg of the prepared catalyst or Pt / C (10 wt.%, Pt) and disperse it in a mixture of 100 μL ethanol and 5 wt.% Nafion, and sonicate for 1 h to obtain a uniform catalyst ink.

[0087] (2) Coat 5 μL of the catalyst ink onto the GCE and dry it at room temperature to obtain the working electrode.

[0088] Cyclic voltammetry (CV) was performed in O2-saturated electrolyte with a potential range from -1 to 0.2 V and a scan rate of 10 mV / s. Linear sweep voltammetry (LSV) was performed with the same potential range as CV in O2-saturated electrolyte, at a scan rate of 5 mV / s and a rotation speed of 1600 rpm. All experiments were conducted at room temperature, and all potentials were converted to the RHE scale, i.e.: E(vs.RHE) = E(relative to Hg / HgCl) + E(Hg / HgCl reference) + 0.0592 pH.

[0089] Application Example 2

[0090] An application of a Co-modified RuO2 catalyst was described, with electrochemical testing conducted in a 0.1 M KOH aqueous solution electrolyte using an electrochemical workstation (CHI1760E, Shanghai) with a typical three-electrode system. A Pt wire electrode and a saturated calomel electrode served as the counter and reference electrodes, respectively. A rotating disk electrode (RDE) with a 4.0 mm diameter glassy carbon electrode (GCE) was used as the working substrate electrode.

[0091] (1) Weigh 10 mg of the prepared catalyst or Pt / C (10 wt.%, Pt) and disperse it in a mixture of 100 μL ethanol and 5 wt.% Nafion, and sonicate for 1 h to obtain a uniform catalyst ink.

[0092] (2) Coat 10 μL of the catalyst ink onto the GCE and dry it at room temperature to obtain the working electrode.

[0093] Application Example 3

[0094] An application of a Co-modified RuO2 catalyst was described, with electrochemical testing conducted in a 0.1 M KOH aqueous solution electrolyte using an electrochemical workstation (CHI1760E, Shanghai) with a typical three-electrode system. A Pt wire electrode and a saturated calomel electrode served as the counter and reference electrodes, respectively. A rotating disk electrode (RDE) with a 4.0 mm diameter glassy carbon electrode (GCE) was used as the working substrate electrode.

[0095] A catalyst ink was prepared by mixing 50 μL of 5 wt% Nafion (Aldrich), 1 ml of ethanol, and 5 mg of Co-SA / RuO2-UNS powder. This ink was then coated onto a composite substrate (1 cm × 1 cm) as an air cathode. A Celgard 2340 membrane (a 38 μm microporous three-layer membrane with a polyethylene layer between two polypropylene layers) was used as a separator to prevent physical contact between the cathode and anode. The electrocatalyst dosage was approximately 1.0 mg·cm⁻². Polarization curves were measured at a scan rate of 10 mV s⁻¹. Constant current charge-discharge cycle measurements at a current density of 10 mA cm⁻² were acquired using a CT-2001A testing system. For comparison, a slurry of RuO2 and 20 wt% Pt / C at a mass ratio of 1:1 was drop-added to the composite substrate at a 1 cm⁻² area to ensure a loading of 1 mg cm⁻² for the air cathode. Zinc-air batteries were assembled and applied under the same conditions.

[0096] The above description is merely an exemplary embodiment of this disclosure, but the scope of protection of this disclosure is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this disclosure should be included within the scope of protection of this disclosure. Therefore, the scope of protection of this disclosure should be determined by the scope of the claims.

Claims

1. A method for preparing a Co-modified RuO2 material, characterized in that, Includes the following steps: S1: Weigh 1-10 g of glucose and 0.1-1 g of urea and dissolve them in 5-30 ml of aqueous solution. Stir for 10-50 min to obtain a mixed solution. Add 0.005-0.03 g of cobalt salt and 0.03-0.05 g of ruthenium salt to the mixed solution and continue stirring for 1-3 h until the solution is clear to obtain the preparation solution. Transfer the preparation solution to a hydrothermal reactor, heat it, and then centrifuge to collect the synthesized precursor. The heating process is as follows: the temperature is set to 100-160℃, and the reaction time is 5-10 h; S2: Weigh 0.1-0.5 g of the synthesized precursor and place it in a muffle furnace to calcine at 300-600 °C for 2-12 h to obtain the final sample.

2. The method for preparing a Co-modified RuO2 material according to claim 1, characterized in that, The cobalt salt in S1 is one or more of cobalt nitrate and cobalt chloride.

3. The method for preparing a Co-modified RuO2 material according to claim 1, characterized in that, The ruthenium salt in S1 is bis(pentamethylcyclopentene)ruthenium, ruthenium dicene, or (1,5-cyclooctadiene)ruthenium chloride.

4. A Co-modified RuO2 material prepared by the preparation method according to any one of claims 1-3.

5. An application of the Co-modified RuO2 material according to claim 4, characterized in that, As a negative electrode catalyst in zinc-air batteries.

6. The application according to claim 5, characterized in that, The specific application method includes the following steps: (1) Weigh 5 mg-10 mg of the prepared Co-modified RuO2 material and disperse it in a mixture of 100 μL-150 μL of ethanol and 5 wt% Nafion, and sonicate for 1 h to obtain a uniform catalyst ink. (2) Coat 5 μL-10 μL of the catalyst ink onto the glassy carbon electrode and dry it at room temperature to obtain the working electrode.

Citation Information

Patent Citations

  • Bifunctional oxygen electrocatalyst and preparation and application thereof