A method for fabricating a vertical channel oxide thin film transistor

By fabricating vertical-channel oxide thin-film transistors, the problem of reducing the channel length of traditional oxide thin-film transistors has been solved, achieving submicron-level channel length and high bending stress resistance, which is suitable for high-frequency and high-pixel-density applications in flexible displays and integrated circuits.

CN117637481BActive Publication Date: 2026-11-17BEIJING SUPERSTRING ACAD OF MEMORY TECH +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311568974.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-22
Publication Date
2026-11-17
Estimated Expiration
2043-11-22

AI Technical Summary

Technical Problem

Existing oxide thin-film transistors struggle to achieve submicron-level channel lengths and meet the high bending stress requirements of flexible electronic products. Traditional photolithography tools limit the reduction of channel length, failing to meet the demands of future high-frequency applications and high pixel density.

Method used

A vertical channel structure is adopted, and source/drain electrodes, active layer, gate dielectric and single/double gate electrodes are fabricated on low-resistivity silicon substrate through processes such as magnetron sputtering, evaporation and photolithography. The photolithography process is simplified and combined with annealing to achieve precise control of the channel length.

Benefits of technology

This technology enables the fabrication of oxide thin-film transistors with submicron channel lengths, reducing process costs and enhancing the application potential of flexible electronics. It is suitable for high-frequency and high-pixel-density displays and integrated circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117637481B_ABST
    Figure CN117637481B_ABST
Patent Text Reader

Abstract

This invention discloses a method for fabricating vertical-channel oxide thin-film transistors (VCDs), belonging to the field of integrated circuits. The VCD fabricated by this method includes a low-resistivity silicon substrate, source / drain electrodes, an active layer, a gate dielectric, and a gate electrode. The source / drain electrodes are located on the upper and lower sides of the active layer, respectively. The gate dielectric is located above the source / drain electrodes on the upper side of the active layer and on both sides of the active layer and the source / drain electrodes. Single / double gate electrodes are located on the gate dielectric. This invention involves the fabrication of both single-gate and double-gate VCD structures. The method utilizes conventional techniques such as photolithography, sputtering, atomic layer deposition, and etching, and is expected to achieve large-scale fabrication of VCDs. It is simple, low-cost, and highly operable, possessing significant application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the fields of display and integrated circuits, and specifically relates to a method for fabricating a single / dual gate vertical channel oxide thin film transistor. Background Technology

[0002] Over the past few decades, display technology has undergone tremendous changes, from the initial CRT monitors to today's LCD and OLED displays. Each technological innovation has brought clearer, more realistic colors, and faster response times. As people's demands for high resolution, high contrast, and high refresh rates continue to increase, innovation in display technology is constantly driving societal progress. Thin-film transistors (TFTs) are the core components of display technology. In recent years, oxide TFTs have seen rapid development due to their advantages, including transparency, low cost, low-temperature fabrication processes, and high performance. Sharp first commercialized indium gallium zinc oxide (IGZO) TFTs in 2012, followed by Samsung, LG, and BOE, which also commercialized IGZO TFTs and rapidly expanded their application to mobile phones, tablets, and other fields. In 2019, the fifth-generation IGZO TFT achieved mass production, with a mobility of 15 cm⁻¹. 2 / Vs can drive ultra-high resolution, large-area (85-inch) displays with resolutions up to 8K. Furthermore, due to the unique advantages of oxide thin-film transistors (OTTs), they have attracted significant attention from academia and industry in emerging integrated circuit technologies, such as flexible skin, flexible transparent circuits, 2T0C DRAM, and monolithic 3D integration. Therefore, research on OTTs is crucial for both the display and integrated circuit fields.

[0003] Existing oxide thin-film transistors (TFTs) already meet some practical application requirements in the display and integrated circuit fields in terms of device performance. However, to meet future higher-quality application demands, such as higher operating frequencies, achieving high current with low voltage, and reducing device area to increase pixel density, it is necessary to develop short-channel TFTs. Due to limitations of traditional photolithography tools, channel lengths are difficult to shrink to the submicron scale. Compared with traditional TFT structures, vertical-channel TFTs can accurately control the channel length by adjusting the thickness of the deposited thin film, thus serving as a viable alternative structure for achieving submicron-level channel lengths. Furthermore, compared with traditional TFT structures, vertical-channel TFTs are more resistant to bending stress and have great potential for applications in flexible electronics. Therefore, developing a process technology suitable for fabricating vertical-channel oxide TFTs is an important topic with practical application potential and research value. This patent proposes a method for fabricating vertical-channel oxide TFTs, and the application of this patent has significant value for the future development of flexible displays and integrated circuits in my country. Summary of the Invention

[0004] The purpose of this invention is to provide a method for fabricating single / dual gate vertical channel oxide thin film transistors, which are mainly applied in the display and integrated circuit fields.

[0005] The technical solution of this invention is:

[0006] A method for fabricating a vertical channel oxide thin-film transistor (VLTT), characterized in that the VLTT comprises, from bottom to top, source / drain electrodes, an active layer, source / drain electrodes, a gate dielectric, and a single / double gate electrode. The source / drain electrodes are located on the upper and lower sides of the active layer, respectively. The gate dielectric is located above the source / drain electrodes on the upper side of the active layer and on both sides of the active layer and the source / drain electrodes. The single / double gate electrode is located above the gate dielectric. The specific steps are as follows:

[0007] 1) Deposit source / drain electrode films on a low-resistivity silicon substrate using magnetron sputtering or vapor deposition processes;

[0008] 2) An active oxide layer is deposited on the source / drain electrodes using magnetron sputtering or atomic layer deposition.

[0009] 3) Deposit source / drain electrode films on the substrate using magnetron sputtering or vapor deposition processes;

[0010] 4) Define the source / drain electrodes and active layer patterns using photolithography or electron beam lithography.

[0011] 5) Use dry etching or wet etching processes to form source / drain electrodes and active layer structures;

[0012] 6) Deposit gate dielectric thin films using plasma-enhanced chemical vapor deposition (PECVD) or atomic layer deposition (ALD).

[0013] 7) Deposit single / dual gate electrode films on the gate dielectric using magnetron sputtering or vapor deposition processes;

[0014] 8) Define the gate dielectric and single / dual gate electrode patterns using photolithography or electron beam lithography.

[0015] 9) Use dry etching or wet etching processes to form the gate dielectric and single / dual gate electrode structure;

[0016] 10) Anneal the vertical channel thin-film transistor to obtain the final thin-film transistor device.

[0017] Furthermore, the source / drain electrode is one or more of the following metals: copper, aluminum, titanium, molybdenum, platinum, gold, silver, etc.; or one or more of the following transparent conductive electrodes: indium tin oxide, aluminum zinc oxide, indium zinc oxide, etc.; or a combination of multiple metal electrodes and transparent conductive electrodes. The thickness of the source / drain electrode is 100 to 500 nanometers.

[0018] Furthermore, the active layer is one or more of zinc oxide, indium oxide, tin oxide, or doped zinc oxide, indium oxide, or tin oxide oxide thin films, and the thickness of the active layer is 5–200 nanometers. For doped zinc oxide, indium oxide, or tin oxide oxide thin films, the doping element is one or more of the following metal elements: aluminum, tin, molybdenum, titanium, hafnium, indium, gallium, etc.; inorganic non-metallic elements: silicon, carbon, phosphorus, etc.; or rare earth elements: lanthanum, erbium, etc. The content of the doping element in the doped zinc oxide, indium oxide, or tin oxide thin films is 0.1%–50%.

[0019] Furthermore, the gate dielectric is one or more of the inorganic insulating thin films such as silicon oxide, silicon nitride, aluminum oxide, hafnium oxide, titanium oxide, and zirconium oxide, and the thickness of the gate dielectric is 5 to 200 nanometers.

[0020] Furthermore, the gate electrode is one or more of the following metals: copper, aluminum, titanium, molybdenum, platinum, gold, silver, etc.; or one or more of the following transparent conductive electrodes: indium tin oxide, aluminum zinc oxide, indium zinc oxide, etc.; or a combination of multiple metal electrodes and transparent conductive electrodes. The thickness of the gate electrode is 5 to 200 nanometers.

[0021] Furthermore, the annealing atmosphere is a vacuum, oxygen, or air, the annealing temperature is 100–300°C, and the annealing time is 1–2 hours.

[0022] The beneficial effects of this invention are:

[0023] (i) This invention makes full use of the characteristics of vertical channel oxide thin film transistors. The channel length of the active layer is defined by the thickness of the active layer, which can realize the fabrication of submicron-sized short channel oxide transistors.

[0024] (ii) This invention involves only two photolithography steps. The active layer and source / drain electrodes are patterned using the same photolithographic mask, and the gate dielectric and gate electrode are patterned using the same photolithographic mask. The steps are simple, highly controllable, and greatly reduce the process cost.

[0025] (III) This invention can realize a dual-gate transistor without adding any process steps, and has great application potential in the field of new integrated circuits. Attached Figure Description

[0026] Figure 1 This is a schematic cross-sectional view of the vertical channel oxide thin film transistor prepared according to the present invention.

[0027] Figure 2 This is a schematic diagram of the process flow for the single-gate and dual-gate vertical channel oxide thin film transistors prepared according to the present invention.

[0028] Figure 3 for Figures 1-2 Legend of the diagram. Detailed Implementation

[0029] The present invention will be further described below with reference to the accompanying drawings and examples. It should be noted that the purpose of disclosing the embodiments is to help further understand the present invention; however, those skilled in the art will understand that various substitutions and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the present invention should not be limited to the content disclosed in the embodiments, and the scope of protection of the present invention is defined by the claims.

[0030] Figure 1 The diagram shows the device structure of a vertical channel oxide thin film transistor prepared using the present invention, including a low-resistivity silicon substrate, source / drain electrodes, an active layer, a gate dielectric, and a gate electrode. The source / drain electrodes are located on the upper and lower sides of the active layer, respectively. The gate dielectric is located on the source / drain electrodes on the upper side of the active layer and on both sides of the active layer and the source / drain electrodes. (a) is a single-gate structure, and (b) is a double-gate structure, with the single / double gate electrodes located on the gate dielectric.

[0031] Figure 2 The diagram illustrates the fabrication process of a vertical-channel oxide thin-film transistor. Taking a low-resistivity silicon substrate, aluminum thin films as the gate electrode and source / drain electrodes, aluminum oxide as the gate dielectric, and zinc oxide as the active layer as an example, the specific fabrication process includes the following steps:

[0032] 1) The low-resistivity silicon substrate was ultrasonically cleaned in acetone, anhydrous ethanol, and deionized water in sequence for 10 minutes.

[0033] 2) A thin aluminum film with a thickness of 100 nanometers is deposited on a single-crystal silicon substrate using a magnetron sputtering process;

[0034] 3) A zinc oxide thin film is deposited using atomic layer deposition (ALD) technology, wherein the zinc oxide thin film has a thickness of 30 nanometers;

[0035] 4) A thin aluminum film is deposited using a magnetron sputtering process, wherein the thickness of the aluminum film is 100 nanometers;

[0036] 5) Use photolithography to define the source / drain electrodes and active layer patterns;

[0037] 6) The aluminum source / drain electrodes and zinc oxide active layer patterns are formed using a wet etching process;

[0038] 7) An alumina film is deposited using atomic layer deposition (ALD) technology, wherein the alumina film has a thickness of 30 nanometers.

[0039] 8) A thin aluminum film is deposited using a magnetron sputtering process, wherein the thickness of the aluminum film is 100 nanometers.

[0040] 9) Use photolithography to define the gate dielectric and gate electrode patterns;

[0041] 10) The aluminum oxide gate dielectric and aluminum gate electrode pattern are formed using a wet etching process;

[0042] 11) The transistors were annealed using a vacuum tube furnace at a temperature of 100 degrees Celsius for 1 hour in an air atmosphere.

[0043] While the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the invention. Any person skilled in the art can make many possible variations and modifications to the technical solutions of the present invention, or modify them into equivalent embodiments, without departing from the scope of the present invention. Therefore, any simple modifications, equivalent changes, and modifications made to the above embodiments based on the technical essence of the present invention, without departing from the scope of the present invention, shall still fall within the protection scope of the present invention.

Claims

1. A method for fabricating a vertical channel oxide thin-film transistor, characterized in that, The vertical channel oxide thin-film transistor (VLT) consists of, from bottom to top, source / drain electrodes, an active layer, source / drain electrodes, a gate dielectric, and single / double gate electrodes. The source / drain electrodes are located on the top and bottom sides of the active layer, respectively. The gate dielectric is located above the source / drain electrodes on the upper side of the active layer and on both sides of the active layer and the source / drain electrodes. The single / double gate electrodes are located above the gate dielectric. The source / drain electrodes are one or more of copper, aluminum, titanium, molybdenum, platinum, gold, and silver; or one or more of indium tin oxide, aluminum zinc oxide, and indium zinc oxide transparent conductive electrodes; or a combination of multiple metal electrodes and transparent conductive electrodes. The active layer is zinc oxide, indium oxide, tin oxide, or one or more of zinc oxide-doped, indium oxide-doped, and tin oxide-doped oxide semiconductor thin films. The semiconductor thin film is doped with zinc oxide, indium oxide, or tin oxide. The doping element is aluminum, tin, molybdenum, titanium, hafnium, indium, or gallium; or silicon, carbon, or phosphorus; or lanthanum or erbium rare earth elements, or a combination thereof. The content of the doping element is 0.1% to 50%. The gate dielectric is one or more of silicon oxide, silicon nitride, aluminum oxide, hafnium oxide, titanium oxide, or zirconium oxide inorganic insulating film. The gate electrode is one or more of copper, aluminum, titanium, molybdenum, platinum, gold, or silver; or one or more of indium tin oxide, aluminum zinc oxide, or indium zinc oxide transparent conductive electrodes; or a combination of multiple metal electrodes and transparent conductive electrodes. The specific steps of the preparation method are as follows: 1) Deposit source / drain electrode films on a low-resistivity silicon substrate using magnetron sputtering or vapor deposition processes; 2) An active oxide layer is deposited on the source / drain electrodes using magnetron sputtering or atomic layer deposition. 3) Deposit source / drain electrode films on the substrate using magnetron sputtering or evaporation processes; 4) Define the source / drain electrodes and active layer patterns using photolithography or electron beam lithography. 5) Use dry etching or wet etching processes to form source / drain electrodes and active layer structures; 6) Deposit gate dielectric thin films using plasma-enhanced chemical vapor deposition (PECVD) or atomic layer deposition (ALD). 7) Deposit single / double gate electrode films on the gate dielectric using magnetron sputtering or vapor deposition processes; 8) Define the gate dielectric and single / dual gate electrode patterns using photolithography or electron beam lithography. 9) Use dry etching or wet etching processes to form the gate dielectric and single / dual gate electrode structure; 10) Anneal the vertical channel thin-film transistor to obtain the thin-film transistor device.

2. The method for fabricating a vertical channel oxide thin-film transistor as described in claim 1, characterized in that, The thickness of the source / drain electrodes is 100~500 nanometers.

3. The method for fabricating a vertical channel oxide thin-film transistor as described in claim 1, characterized in that, The active layer has a thickness of 5-200 nanometers.

4. The method for fabricating a vertical channel oxide thin-film transistor as described in claim 1, characterized in that, The thickness of the gate dielectric is 5~200 nanometers.

5. The method for fabricating a vertical channel oxide thin-film transistor as described in claim 1, characterized in that, The thickness of the gate electrode is 5~200 nanometers.

6. The method for fabricating a vertical channel oxide thin-film transistor as described in claim 1, characterized in that, The annealing process is carried out in a vacuum, oxygen, or air atmosphere, at a temperature of 100-300°C, and for 1-2 hours.

Citation Information

Patent Citations

  • Preparation method of nanoscale oxide transistor

    CN116404045A

  • Thin film transistor and method of manufacturing the same

    KR1020180025882A