A supported Pd-based selective hydrogenation catalyst and its preparation method and application
By preparing Pd@C core-shell nanoparticles on a carbon material support, the problem of dechlorination of Pd-based catalysts in the hydrotreating of p-chloronitrobenzene is solved, and a catalytic effect with high selectivity and environmental protection is achieved.
Patent Information
- Application Number
- CN202311587273.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-24
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-11-24
AI Technical Summary
The existing Pd-based hydrogenation catalysts have side-effects of dechlorination in the p-chloronitrobenzene hydrogenation reaction, and the chemical reduction reagents and hydrogen used in the preparation process are harmful to the environment, making it difficult to improve the dispersion of metal Pd while increasing the dispersion of metal. Selectivity of chloroaniline.
Using high specific surface area carbon material as a carrier, through impregnation, grinding and calcining steps, environmentally friendly organic molecules and nitrogen-containing molecules replace the reinforcement reduction reagent, Pd@C core shell with small particle size and uniform particle size distribution is prepared. Nanoparticles inhibit side reactions of dechlorination.
The high conversion rate of p-chloronitrobenzene and 100% selectivity of p-chloroaniline are achieved, which avoids the occurrence of side reactions of dechlorination, and the preparation process is environmentally friendly and the use of toxic reagents are avoided.
Smart Images

Figure HDA0004570234870000011 
Figure HDA0004570234870000021 
Figure HDA0004570234870000031
Abstract
Description
Technical Field
[0001] The invention relates to a Pd-based selective hydrogenation catalyst and a preparation method thereof and application of the catalyst in a p-chloronitrobenzene (p-CNB) hydrogenation reaction. Background Art
[0002] p-Chloroaniline is an important chemical intermediate, which is widely used in the production of fine chemical products such as medicine, pesticides, textile dyes, etc., and has a huge market demand. p-Chloroaniline is generally prepared by reducing p-chloronitrobenzene. Among various reduction methods, catalytic hydrogenation has attracted widespread attention from researchers due to its simple process and environmental friendliness. Catalytic hydrogenation reduction method refers to dissolving p-chloronitrobenzene in a solvent such as ethanol, adding a catalyst, and then passing hydrogen at a certain temperature for catalytic hydrogenation to reduce the nitro group to an amino group to obtain p-chloroaniline.
[0003] Among the various catalysts suitable for the catalytic hydrogenation of p-chloronitrobenzene (p-CNB), Pd-based catalysts have the advantages of high reactivity and mild reaction conditions, but they are expensive and prone to dechlorination side reactions during the hydrogenation reaction, which not only reduces the yield and purity of the product, but also the strong acid produced during the reaction will cause pollution and corrosion to the reaction equipment. In order to inhibit the dechlorination side reaction during the hydrogenation reaction, the commonly used methods are: 1) adding various organic dechlorination inhibitors during the reaction [CN109369414, CN103242168]; 2) adding various additives to modulate the electronic and geometric properties of the Pd active center [CSLu, et al. ACS Sustainable Chemistry & Engineering. 2019, 7, 8542-8553]; 3) modulating the interaction between Pd and the carrier [HMLiu, et al. Catalysis Science & Technology. 2015, 5 (1): 405-414]. At the same time, improving the dispersion of metal Pd particles is an important method to improve the activity of supported Pd-based catalysts. However, existing research results show that the preparation of Pd-based catalysts with high dispersion characteristics often requires the use of strong chemical reducing agents such as sodium borohydride [C-GJessica, et al. ACS Sustainable Chemistry & Engineering, 2020, 8(39): 15030-15043] or the use of hydrogen for reduction at high temperature to prepare Pd / C catalysts [Chinese Patent CN 115970723 A]; and as the dispersion of metal Pd particles increases, the selectivity of Pd-based catalysts for p-chloroaniline (p-CAN) also decreases [JHLyu, et al. The Journal of Physical Chemistry C, 2014, 118(5): 2594-2601]. Therefore, how to improve the dispersion of metal Pd while suppressing the dechlorination side reaction to improve the selectivity of p-CAN products, and using environmentally friendly reagents to replace hydrogen or strong reducing reagents to prepare supported metal Pd catalysts are the key contents of the current research and development of Pd-based hydrogenation catalysts.
[0004] In order to solve the difficulties encountered in the development of the above-mentioned Pd-based hydrogenation catalyst, the present invention patent reports a new method for preparing a Pd-based hydrogenation catalyst using a high specific surface area carbon material as a carrier and its application in the p-CNB hydrogenation reaction. Environmentally friendly organic molecules and nitrogen-containing molecules are used instead of strong chemical reducing agents such as sodium borohydride. Through preparation steps such as impregnation, grinding and calcination, Pd@C core-shell nanoparticles with small metal Pd particle size and uniform particle size distribution can be prepared directly on the carbon carrier. In the hydrogenation reaction of p-chloronitrobenzene, the p-CNB conversion rate and p-CAN selectivity of the Pd-based catalyst can reach ~100%, successfully suppressing the occurrence of dechlorination side reactions. Summary of the invention
[0005] In order to solve the problems of 1) using toxic and harmful reducing agents to the environment in the existing preparation methods of supported Pd-based selective hydrogenation catalysts, and 2) the existence of a dechlorination side reaction in the hydrogenation reaction of p-chloronitrobenzene caused by highly dispersed Pd particles in the supported Pd-based selective hydrogenation catalyst, the present invention provides a supported Pd-based selective hydrogenation catalyst, a preparation method thereof, and application in the hydrogenation reaction of p-chloronitrobenzene. A high specific surface area carbon material is used as a carrier, and environmentally friendly organic molecules and nitrogen-containing molecules are used. Through the steps of impregnation, grinding and calcination, Pd@C core-shell nanoparticles with small metal Pd particle size and uniform particle size distribution are directly prepared on the carbon carrier. The Pd-based catalyst is used in the catalytic hydrogenation reaction of p-chloronitrobenzene, and not only has high reaction activity, but also suppresses the dechlorination side reaction.
[0006] The technical solutions adopted to solve the above technical problems are described below.
[0007] In a first aspect, the present invention provides a method for preparing a supported Pd-based selective hydrogenation catalyst, the preparation method comprising the following steps:
[0008] (a) The specific surface area shall not be less than 1400m 2 / g of carbon material is added into a nitric acid solution for reflux treatment, and then filtered, washed and dried to obtain the desired carbon carrier A;
[0009] (b) obtaining a mixed aqueous solution B of a palladium-containing inorganic salt and polyethylene glycol, wherein the mass ratio of the palladium-containing inorganic salt to the organic molecule is 1.2-1.6, preferably 1.4-1.6; and the molecular weight of the polyethylene glycol is 1000-2000;
[0010] (c) adding the mixed aqueous solution B dropwise to the carbon support A and mixing and stirring, and sequentially performing room temperature impregnation, water bath treatment, and oven drying to obtain a precursor D, wherein the ratio of the mass of palladium in the mixed aqueous solution B to the mass of the carbon support A is 0.2-1.0 wt %;
[0011] (d) Precursor D is calcined at high temperature to obtain a supported Pd-based selective hydrogenation catalyst.
[0012] In step (a) of the present invention, the number of oxygen-containing functional groups on the surface of the carbon material is regulated by treating the carbon material with nitric acid. Preferably, the mass fraction of the nitric acid solution is 28-56wt%, and the mass ratio of the nitric acid solution to the carbon material is 7-8:1; more preferably, the mass fraction of the nitric acid solution is 28wt%, and the mass ratio of the nitric acid solution to the carbon material is 7.5:1. Preferably, the reflux treatment temperature in step (a) is 70-80°C, more preferably 80°C, the magnetic stirring is 400-600r / min, more preferably 500r / min, and the reflux treatment time is 3-4h, more preferably 4h.
[0013] In step (b) of the present invention, the addition of polyethylene glycol forms a thin film carbon shell during the calcination process, and the formation of the thin film carbon shell helps to suppress the dechlorination side reaction in the hydrogenation reaction of p-chloronitrobenzene under the catalysis of the supported Pd-based selective hydrogenation catalyst, and significantly improves the selectivity of the target product p-chloroaniline. Considering that the presence of the thin film carbon shell in the catalyst will reduce the activity of the catalyst, the polyethylene glycol is preferably selected, and polyethylene glycol-1000 is selected. Selecting this polyethylene glycol can significantly improve the selectivity of p-chloroaniline, but the catalytic activity is only slightly reduced.
[0014] In step (c) of the present invention, the room temperature impregnation is preferably room temperature impregnation to ensure uniform dispersion of Pd, and the palladium element concentration and volume dosage in the mixed aqueous solution C can be determined according to the required palladium loading (i.e., the mass ratio of palladium to carbon carrier A). In the specific configuration process of the mixed aqueous solution B, an aqueous solution of a palladium-containing inorganic salt and an aqueous solution of polyethylene glycol can be first configured, and then the two are mixed in proportion to form a mixed aqueous solution B. The palladium-containing inorganic salt can be at least one of palladium nitrate dihydrate, palladium chloride, and palladium sulfate.
[0015] Preferably, the room temperature immersion time in step (c) is 3-4 hours, more preferably 4 hours.
[0016] Preferably, the water bath treatment conditions in step (c) are: the water bath temperature is 70-80° C., more preferably 80° C., and the water bath time is 0.5-1 h, more preferably 1 h.
[0017] Preferably, the oven drying conditions in step (c) are: oven drying temperature is 100-110° C., more preferably 100° C.; and drying time is 3-4 h, more preferably 4 h.
[0018] Preferably, in step (d), the high temperature calcination treatment conditions are: calcination is carried out under the protection of inert gas, the calcination temperature is 400-500°C, more preferably 400°C, and the calcination time is 4-5h, more preferably 4h.
[0019] Preferably, in step (d), the precursor D and glycine are mixed before high-temperature calcination, and the mixture is ground evenly before high-temperature calcination, wherein the mass ratio of glycine to carbon carrier A is 0.01-0.06:3, more preferably 0.01:3. Glycine decomposes during high-temperature calcination to dope nitrogen into the activated carbon, which synergizes with polyethylene glycol to improve the selectivity of the target product while ensuring the activity of the Pd catalyst.
[0020] As further preferred, in step (d), the grinding method is manual grinding in an agate mortar, and the grinding time is 20-30 min, more preferably 30 min.
[0021] As a further preference, in step (d), the high temperature calcination is carried out in a high purity nitrogen atmosphere (99.999%), the calcination temperature is 400° C., and the calcination time is 4 hours.
[0022] In a second aspect, the present invention provides a supported Pd-based selective hydrogenation catalyst prepared according to the preparation method described in the first aspect. The supported Pd-based catalyst is composed of a carbon support and palladium-containing nanoparticles uniformly supported on the surface of the nitrogen-doped carbon support, wherein the particle size of the palladium-containing nanoparticles is 2-6 nanometers and has a Pd@C core-shell structure, wherein the palladium element is Pd 0 .
[0023] Preferably, the carbon carrier is a nitrogen-doped carbon carrier.
[0024] In a third aspect, the present invention provides an application of the supported Pd-based catalyst in the catalytic hydrogenation reaction of p-chloronitrobenzene. The Pd-based catalyst exhibits excellent reaction activity and selectivity for the p-chloroaniline product during the catalytic hydrogenation reaction of p-chloronitrobenzene.
[0025] Compared with the prior art, the present invention has the following advantages:
[0026] (1) The Pd-based catalyst reported in the present invention only requires simple impregnation, grinding, and calcination steps, and the preparation process is simple and does not require complex instruments and equipment.
[0027] (2) The Pd-based catalyst preparation process reported in the present invention does not use toxic, environmentally hazardous strong reducing agents or hydrogen reduction, and the preparation process is green and environmentally friendly.
[0028] (3) The Pd-based catalyst reported in the present invention has excellent catalytic reaction performance in the catalytic hydrogenation reaction of p-chloronitrobenzene, showing excellent reaction activity and product selectivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 and Figure 2 is a TEM image of the catalyst prepared in Example 2.
[0030] Figure 3 is the XRD pattern of the catalyst prepared in Example 2.
[0031] Figure 4 This is the XPS graph of the catalyst prepared in Example 2. DETAILED DESCRIPTION
[0032] The technical scheme of the present invention is further described below with specific examples, but the protection scope of the present invention is not limited thereto: Example 1 (without glycine)
[0033] Take 64.62g of 65-68wt% HNO3 solution, add 85.38g of deionized water, prepare 28wt% nitric acid solution and mix with 20g of carbon material (Jiangsu Xinghong Carbon Technology Co., Ltd., specific surface area 1598.8m 2 / g, pore volume 0.87cm 3 / g) mixed. After reflux treatment at 80°C for 4h with magnetic stirring (500r / min), cool to room temperature, and then wash with deionized water until the filtrate pH is ≈ 7. The treated carbon material is placed in an oven and dried at 100°C for 12h. Weigh 0.1750g PEG-1000 into a beaker, add 3mL deionized water to make solution A. Take 1.5mL of palladium nitrate solution (mix 0.2590 grams of palladium nitrate dihydrate with 10mL deionized water) and add it to 1.5mL deionized water, stir evenly, and make solution B. Mix solution A and solution B evenly, then add dropwise to 3.0g (200-300 mesh) of carbon support and impregnate at room temperature for 4h. After being treated in an 80°C water bath for 1h, place in a 100°C oven and dry for 4h. The sample was placed in a tube furnace and calcined under N2 atmosphere (99.999%, N2 flow rate of 100 mL / min) at 400°C for 4 h. The 0.5-Pd / AC-PEG catalyst was obtained when the temperature was cooled to room temperature.
[0034] Embodiment 2:
[0035] Take 64.62g of 65-68wt% HNO3 solution, add 85.38g of deionized water, prepare 28wt% nitric acid solution and mix with 20g of carbon material (Jiangsu Xinghong Carbon Technology Co., Ltd., specific surface area 1598.8m2 / g, pore volume 0.87cm 3 / g) mixed. After reflux treatment at 80°C for 4h with magnetic stirring (500r / min), cool to room temperature, and then wash with deionized water until the filtrate pH is ≈ 7. The treated carbon material is placed in an oven and dried at 100°C for 12h. Weigh 0.1750g PEG-1000 into a beaker, add 3mL deionized water to make solution A. Take 1.5mL of palladium nitrate solution (mix 0.2590 grams of palladium nitrate dihydrate with 10mL deionized water) and add it to 1.5mL deionized water, stir evenly, and make solution B. Mix solution A and solution B evenly, then add dropwise to 3.0g (200-300 mesh) of carbon support and impregnate at room temperature for 4h. After being treated in an 80°C water bath for 1h, place in a 100°C oven and dry for 4h. 0.01 g of glycine was added to the dried sample and ground in an agate mortar for 30 min. The sample was placed in a tube furnace and calcined under N2 atmosphere (99.999%, N2 flow rate of 100 mL / min) at 400°C for 4 h. When it cooled to room temperature, 0.5-Pd / AC-PEG-0.01G catalyst was obtained.
[0036] like Figure 1 and Figure 2 As shown, the lattice fringe spacing of the particles in the catalyst is It corresponds to the metallic Pd (111) crystal plane (JCPDS No.87-0637) and has an obvious core-shell structure with uniformly distributed particles. Figure 3 The XRD characterization diagram of the catalyst shows that a weak diffraction peak appears near 2θ≈39°, which can be attributed to the metal Pd (111) crystal plane (JCPDS No.87-0637). XRD characterization shows that Pd 0 The particle size of the palladium-containing particles in the catalyst was estimated to be about 4.9 nm using the Scherrer equation. Figure 4 N as catalyst 1s XPS spectrum. As shown in the figure, a N 1s The XPS peaks can be attributed to pyrrolic nitrogen species, indicating that the carbon material was successfully doped with nitrogen.
[0037] Comparative Example 1 (without addition of organic matter and glycine)
[0038] Take 64.62g of 65-68wt% HNO3 solution, add 85.38g of deionized water, prepare 28wt% nitric acid solution and mix with 20g of carbon material (Jiangsu Xinghong Carbon Technology Co., Ltd., specific surface area 1598.8m 2 / g, pore volume 0.87cm3 / g). After being refluxed for 4 hours under 80°C temperature conditions with magnetic stirring (500r / min), it was cooled to room temperature and then washed with deionized water until the pH of the filtrate was ≈7. The treated carbon material was placed in an oven and dried for 12 hours at 100°C. Take 3mL of deionized water to make solution A. Take 1.5mL of palladium nitrate solution (mix 0.2590 grams of palladium nitrate dihydrate with 10mL of deionized water) and add it to 1.5mL of deionized water, stir evenly, and make solution B. Solution A and solution B were mixed evenly, and then added dropwise to 3.0g (200-300 mesh) of carbon carrier and impregnated at room temperature for 4h. After being treated in an 80°C water bath for 1h, it was placed in a 100°C oven and dried for 4h. The sample was placed in a tubular furnace and calcined under N2 atmosphere conditions (99.999%, N2 flow rate of 100mL / min), the calcination temperature was 400°C, and the calcination time was 4h. After the temperature is cooled to room temperature, 0.5-Pd / AC-PEG-free catalyst is obtained.
[0039] Comparative Example 2 (Adding PEG-2000)
[0040] Take 64.62g of 65-68wt% HNO3 solution, add 85.38g of deionized water, prepare 28wt% nitric acid solution and mix with 20g of carbon material (Jiangsu Xinghong Carbon Technology Co., Ltd., specific surface area 1598.8m 2 / g, pore volume 0.87cm 3 / g) mixed. After being refluxed for 4 hours under magnetic stirring (500r / min) at 80°C, it was cooled to room temperature and then washed with deionized water until the pH of the filtrate was ≈7. The treated carbon material was placed in an oven and dried for 12 hours at 100°C. Weigh 0.1750g PEG-2000 into a beaker, add 3mL deionized water to make solution A. Take 1.5mL of palladium nitrate solution (mix 0.2590 grams of palladium nitrate dihydrate with 10mL deionized water) and add it to 1.5mL deionized water, stir evenly, and make solution B. Mix solution A and solution B evenly, then add dropwise to 3.0g (200-300 mesh) of carbon support and impregnate at room temperature for 4 hours. After being treated in an 80°C water bath for 1 hour, place it in a 100°C oven and dry it for 4 hours. The sample was placed in a tube furnace and calcined under N2 atmosphere (99.999%, N2 flow rate of 100 mL / min) at 400°C for 4 h. The 0.5-Pd / AC-PEG-2000 catalyst was obtained after cooling to room temperature.
[0041] Comparative Example 3 (addition of glycine without addition of organic matter)
[0042] Take 64.62g of 65-68wt% HNO3 solution, add 85.38g of deionized water, prepare 28wt% nitric acid solution and mix with 20g of carbon material (Jiangsu Xinghong Carbon Technology Co., Ltd., specific surface area 1598.8m 2 / g, pore volume 0.87cm 3 / g) mixed. After being refluxed for 4 hours under magnetic stirring (500r / min) at 80°C, it was cooled to room temperature and then washed with deionized water until the pH of the filtrate was ≈7. The treated carbon material was placed in an oven and dried at 100°C for 12 hours. Take 3mL of deionized water to make solution A. Take 1.5mL of palladium nitrate solution (mix 0.2590 grams of palladium nitrate dihydrate with 10mL of deionized water) and add it to 1.5mL of deionized water, stir evenly, and make solution B. Mix solution A and solution B evenly, then add dropwise to 3.0g (200-300 mesh) of carbon carrier and impregnate at room temperature for 4 hours. After being treated in an 80°C water bath for 1 hour, place it in a 100°C oven and dry it for 4 hours. 0.01 g of glycine was added to the dried sample and ground in an agate mortar for 30 min. The sample was placed in a tube furnace and calcined under N2 atmosphere (99.999%, N2 flow rate of 100 mL / min) at 400°C for 4 h. When it cooled to room temperature, 0.5-Pd / AC-PEG-free-0.01G catalyst was obtained.
[0043] Embodiment 3:
[0044] A stainless steel high pressure reactor (100 cm 3 ) The Pd-based catalysts prepared by Comparative Example 1, Comparative Example 2, Comparative Example 3, Example 1, and Example 2 were subjected to a p-chloronitrobenzene catalytic hydrogenation reaction performance evaluation test experiment. First, 50 mL of anhydrous ethanol, 1.0 g of p-CNB, and 0.05 g of catalyst were added to a high-pressure reactor. Before the reaction, the reactor system was first replaced with high-purity H2 (99.999%) for 6 times, and then the hydrogenation reaction was carried out under magnetic stirring (1000 rpm), 333 K, and 1.1 MPa. The hydrogenation products were qualitatively and quantitatively analyzed using a gas chromatograph (Agilent GC7890B) equipped with a flame ionization detector.
[0045] The results of the hydrogenation experiments show that the time for p-CNB to reach 100% conversion is 60 minutes using the 0.5-Pd / AC-PEG-free (PEG-1000 not added) catalyst prepared in Comparative Example 1, but the product contains dechlorinated byproduct aniline (aniline selectivity is 5.7%, p-CAN selectivity is 94.3%). The time for p-CNB to reach 100% conversion is 120 minutes using the 0.5-Pd / AC-PEG-2000 (PEG-2000 added) catalyst prepared in Comparative Example 2. The p-CAN selectivity is 100% using the 0.5-Pd / AC-PEG (PEG-1000 added) catalyst prepared in Example 1, but the time for p-CNB to reach 100% conversion is 90 minutes. Using the 0.5-Pd / AC-PEG-free-0.01G (no PEG added but glycine added) catalyst prepared in Comparative Example 3, the time to reach 100% conversion of p-CNB was 60 minutes, but the product contained dechlorinated byproduct aniline (aniline selectivity was 6.8%, p-CAN selectivity was 93.2%). Using the 0.5-Pd / AC-PEG-0.01G catalyst prepared in Example 2, the time to reach 100% conversion of p-CNB was 60 minutes, and the p-CAN selectivity was 100%.
[0046] The above experimental results show that the method shown in the present invention can be used to prepare a Pd-based catalyst without using a strong chemical reducing agent or high-temperature H2 reduction. The p-CNB conversion rate and p-CAN selectivity of the Pd-based catalyst can reach 100%, successfully suppressing the occurrence of dechlorination side reactions. Therefore, the Pd-based catalyst reported in the present invention has excellent catalytic reaction performance in the catalytic hydrogenation reaction of p-chloronitrobenzene, showing excellent reaction activity and product selectivity.
Claims
1. A method for preparing a supported Pd-based selective hydrogenation catalyst, characterized in that: The preparation method comprises the following steps: (a) The specific surface area shall not be less than 1400m 2 / g of carbon material is added into a nitric acid solution for reflux treatment, and then filtered, washed and dried to obtain the desired carbon carrier A; (b) obtaining a mixed aqueous solution B of a palladium-containing inorganic salt and polyethylene glycol, wherein the mass ratio of the palladium-containing inorganic salt to the organic molecule is 1.2-1.6; and the molecular weight of the polyethylene glycol is 1000; (c) adding the mixed aqueous solution B dropwise to the carbon support A and mixing and stirring, and sequentially performing room temperature impregnation, water bath treatment, and oven drying to obtain a precursor D, wherein the ratio of the mass of palladium in the mixed aqueous solution B to the mass of the carbon support A is 0.2-1.0 wt %; (d) The precursor D is subjected to high temperature calcination to obtain a supported Pd-based selective hydrogenation catalyst, wherein the calcination is carried out under the protection of an inert gas.
2. The preparation method according to claim 1, characterized in that: In step (d), the high temperature calcination treatment conditions are: calcination temperature is 400-500° C., and calcination time is 4-5 hours.
3. The preparation method according to claim 2, characterized in that: In step (d), the high temperature calcination treatment conditions are: calcination temperature is 400° C., and calcination time is 4 hours.
4. The preparation method according to claim 2, characterized in that: Step (d) Before high-temperature calcination, the precursor D and glycine are first mixed, ground evenly, and then subjected to high-temperature calcination treatment, wherein the mass ratio of glycine to carbon carrier A is 0.01-0.06:
3.
5. The preparation method according to claim 4, characterized in that: In step (d), the mass ratio of glycine to carbon carrier A is 0.01:
3.
6. The preparation method according to claim 4, characterized in that: In step (d), the grinding method is manual grinding in an agate mortar, and the grinding time is 20-30 minutes.
7. The preparation method according to any one of claims 1 to 6, characterized in that: In step (b), the mass ratio of the palladium-containing inorganic salt to the organic molecule is 1.4-1.
6.
8. The preparation method according to any one of claims 1 to 6, characterized in that: In step (a), the mass fraction of the nitric acid solution is 28-56wt%, and the mass ratio of the nitric acid solution to the carbon material is 7-8:1; the reflux treatment temperature is 70-80°C, the magnetic stirring is 400-600r / min, and the reflux treatment time is 3-4h.
9. The preparation method according to any one of claims 1 to 6, characterized in that: In step (c), the palladium-containing inorganic salt is at least one of palladium nitrate dihydrate, palladium chloride, and palladium sulfate; the room temperature impregnation is room temperature impregnation, and the room temperature impregnation time is 3-4h; the water bath treatment conditions are: the water bath temperature is 70-80°C, and the water bath time is 0.5-1h; the oven drying temperature is 100-110°C, and the drying time is 3-4h.
10. A supported Pd-based selective hydrogenation catalyst prepared according to the preparation method according to any one of claims 1 to 9.
11. Use of the supported Pd-based catalyst as claimed in claim 10 in the catalytic hydrogenation reaction of p-chloronitrobenzene.