A method for charging a smelting furnace capable of improving the first-grade silicon carbide yield

By using microchannel refractory bricks and air guides in silicon carbide smelting furnaces, combining carbon and silicon raw materials distribution with different particle sizes, the problem of impurity gas emissions in the smelting furnaces is solved, product quality and breathability are improved, and product quality and breathability are improved. First-grade rate.

CN117663781BActive Publication Date: 2024-11-01NINGXIA JINHAI XINGSHENG CARBORUNDUM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311669195.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-07
Publication Date
2024-11-01
Estimated Expiration
2043-12-07

AI Technical Summary

Technical Problem

In existing silicon carbide smelting furnaces, the product quality gradually decreases due to the gasification of impurities under high temperature and high pressure, especially the quality of silicon carbide products near the furnace wall, and the insufficient breathability of the sealed smelting furnace leads to a low output rate of excellent products.

Method used

Refractory bricks with microchannels are used as the furnace bottom, the air guide channel is connected to the exhaust gas recovery system, and carbon and silicon raw materials of different particle sizes are set at different furnace cross-sectional positions to form gas emission channels to improve breathability and directional collection is harmful gas.

Benefits of technology

The first-grade product rate of silicon carbide products has been significantly improved, from 48% to 55%, reducing impurity content and ensuring that harmful gases are not emitted into the atmosphere.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117663781B_ABST
    Figure CN117663781B_ABST
Patent Text Reader

Abstract

The present invention provides a method for charging a smelting furnace that can improve the first-grade rate of silicon carbide. A silicon carbide smelting furnace that can improve the first-grade rate of silicon carbide is used. In the charging method, the charging area is divided into a heat preservation material area, a resistance material area, a first area, a second area, a third area, and a fourth area. The first area is the furnace bottom area, the second area is the furnace top area, the third area is the area adjacent to the furnace wall, and the fourth area is other areas in the smelting furnace except the first area, the second area, the third area, the heat preservation material area, and the resistance material area; wherein the particle size of the silicon carbide smelting raw material laid in the first area and the second area is larger than the particle size of the silicon carbide smelting raw material in the third area and the fourth area. In the present application, large-particle materials are laid in the furnace bottom and furnace top areas, so that a gas discharge channel can be formed between the bottom materials, ensuring that harmful gases are discharged smoothly through the microchannels of the refractory brick layer at the bottom of the furnace, thereby improving the first-grade rate of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of a silicon carbide smelting furnace and silicon carbide smelting preparation, in particular to a method for loading a silicon carbide smelting furnace capable of improving the first-grade silicon carbide rate. Background Art

[0002] Silicon carbide smelting furnace is a kind of equipment used for smelting silicon carbide. When smelting silicon carbide, the smelting furnace contains: carbonaceous raw materials and silicon raw materials for smelting silicon carbide, resistance materials for heating, and insulation materials for keeping the furnace body warm.

[0003] The specific process of silicon carbide smelting is as follows:

[0004] a. Starting from about 1700℃, the siliceous raw material changes from sand to melt and then to vapor.

[0005] b. SiO2 melt and vapor penetrate into the pores of the carbon material, infiltrate the carbon particles, and react to form silicon carbide SiC.

[0006] c. When the temperature rises to 1700~1900℃, β-SiC is generated.

[0007] d. When the temperature rises to 1900~2000℃, the fine β-SiC transforms into α-SiC, and the α-SiC crystals gradually grow and become dense, and the growth process continues until 2500℃.

[0008] When the furnace temperature rises to about 2500℃, SiC begins to decompose and turns into silicon vapor and graphite: SiC→Si↑+C. Silicon vapor and carbon in the appropriate temperature range can regenerate new SiC.

[0009] The carbonaceous and silicon raw materials used in silicon carbide smelting contain metal impurities, sulfur, phosphorus and other impurities. During the smelting process, the furnace is in a high temperature and high pressure state, and the impurities in the reaction materials will be gasified at high temperature. Under high temperature and high pressure, the gasified impurities will be discharged around the furnace core. As the temperature from the furnace core to the furnace wall area gradually decreases, these gas impurities will become solid and doped in silicon carbide at a certain temperature, resulting in the poorer quality of silicon carbide products closer to the furnace wall. Summary of the invention

[0010] In order to solve the problems existing in the background technology, the present application provides a silicon carbide smelting furnace and a furnace loading method that can improve the first-grade silicon carbide rate.

[0011] In the first aspect, the present application provides a silicon carbide smelting furnace capable of improving the first-grade silicon carbide yield, comprising a furnace bottom, an environmentally friendly sealed furnace wall surrounded by refractory bricks and sealed with cement, characterized in that the furnace bottom is made of refractory bricks containing microchannels, the microchannels penetrate from the top surface of the refractory bricks to the bottom surface of the refractory bricks, the diameter of the microchannels is 200 μm~300 μm, and the density of the microchannels in the refractory bricks is 300 / cm 2 ~350pcs / cm 2 ;

[0012] The smelting furnace further comprises: an air duct arranged at the lower layer of the furnace bottom, the air duct being composed of through holes arranged transversely on the refractory bricks containing the microchannels, and the air duct being in communication with the microchannels.

[0013] As a preferred technical solution of the present application, the air guide channel is transversely arranged in a refractory brick having a microchannel, and the microchannel is connected to the air guide channel.

[0014] As a preferred technical solution of the present application, the air duct is connected to the exhaust gas recovery system.

[0015] Based on the same inventive concept, the second aspect of the present invention provides a furnace loading method for smelting silicon carbide using the smelting furnace provided by the first aspect, wherein the furnace loading area is divided into a heat preservation material area, a resistance material area, a first area, a second area, a third area, and a fourth area, wherein the first area is the furnace bottom area, the second area is the furnace top area, the third area is the area adjacent to the furnace wall, and the fourth area is other areas in the smelting furnace except the first area, the second area, the third area, the heat preservation material area, and the resistance material area;

[0016] Among them, the particle size of the silicon carbide smelting raw materials laid in the first area and the second area is larger than the particle size of the silicon carbide smelting raw materials laid in the third area and the fourth area.

[0017] The particle size of the silicon carbide smelting raw material laid in the fourth area is larger than the particle size of the silicon carbide smelting raw material laid in the third area.

[0018] The particle size of the carbonaceous raw materials in the silicon carbide smelting raw materials charged to the first area is 3mm-4mm, and the particle size of the silicon raw materials is 6mm-10mm.

[0019] The particle size of the carbonaceous raw material in the silicon carbide smelting raw material charged in the second zone is 3mm to 4mm, and the particle size of the siliceous raw material is 6mm to 10mm;

[0020] The particle size of the carbonaceous raw material in the silicon carbide smelting raw material charged to the third zone is less than 2 mm, and the particle size of the silicon raw material is less than 1 mm;

[0021] The particle size of the carbonaceous raw material in the silicon carbide smelting raw materials loaded into the furnace in the fourth area is 2mm-3mm, and the particle size of the siliceous raw material is 1mm-6mm.

[0022] The carbonaceous raw material is anthracite and the siliceous raw material is silicon dioxide.

[0023] The ratio of siliceous raw materials to carbonaceous raw materials is 1.17~1.19:1.

[0024] The SiO2 content in the siliceous raw material is ≥98%.

[0025] In carbonaceous raw materials, the fixed carbon content is >80% and the ash content is 3% to 10%.

[0026] The beneficial effects of this application are:

[0027] 1. The present invention improves the furnace bottom structure of the existing environmentally friendly sealed furnace. The furnace bottom is paved with refractory bricks with a microchannel structure. The lower layer of the refractory bricks is designed with an air duct connected to the tail gas recovery system. Various gas phase side reaction products generated by the reaction during the silicon carbide smelting process and various harmful metals and metal oxides gasified at high temperature can be discharged from the microchannels at the bottom of the furnace, enter the tail gas recovery system through the air duct, and are discharged after purification. When loading the furnace, the bottom reaction zone area is increased, thereby expanding the superior product reaction zone.

[0028] 2. In the prior art, the particle size of the charge in each part of the silicon carbide furnace is consistent, which is not conducive to the air permeability of the charge when used in a sealed smelting furnace, and the output rate of superior products is low. In the present invention, materials of different particle sizes are laid at different cross-sectional positions in the furnace, and large-particle materials are laid in the furnace bottom and furnace top areas, so that a gas discharge channel can be formed between the bottom materials, ensuring that harmful gases can be discharged smoothly through the microchannels of the refractory brick layer at the bottom of the furnace. Small-particle materials are laid near the furnace wall, so that the harmful gases flowing in this direction are blocked from penetrating and are forced to be discharged upward or downward into the tail gas collection system. This technology significantly improves the air permeability of the sealed smelting furnace, reduces the impurity content of the product, and increases the first-grade rate of the product. At the same time, it can also ensure the directional collection of harmful gases and prevent them from being discharged into the atmosphere.

[0029] Through the present invention, the first-grade rate of silicon carbide products can be increased from 48% to 55%. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a schematic diagram of a silicon carbide smelting furnace for this application;

[0031] Figure 2 This is a schematic diagram of the furnace structure of the silicon carbide smelting furnace of this application;

[0032] Figure 3 This is an axial cross-sectional view of the silicon carbide smelting furnace of the present application;

[0033] Figure 4 For this application Figure 3 The enlarged schematic diagram at A in the middle;

[0034] Figure 5 This is a diagram of the charge distribution for this application and a schematic diagram of the gas flow in the furnace during silicon carbide smelting;

[0035] Figure 6 It is a prior art charge distribution diagram and a schematic diagram of the gas flow in the furnace during silicon carbide smelting;

[0036] In the figure, 1, furnace bottom; 11, refractory bricks; 111, microchannel; 112, air duct; 2, furnace wall; 3, furnace head; 4, exhaust gas recovery system; 41, flue gas collection hood, 42, lower flue gas collection main pipe, 43, lower flue gas channel, 51, first area; 52, second area; 53, third area; 54, fourth area, 55, insulation material area; 56, resistance material area. DETAILED DESCRIPTION

[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0038] The invention relates to a silicon carbide smelting furnace capable of improving the first-grade silicon carbide product rate, and improves the consistency of graphitization process of graphitization raw materials in different areas through furnace loading, power transmission and heat flow during power transmission. Example

[0039] An embodiment of a silicon carbide smelting furnace capable of improving the first-grade silicon carbide yield.

[0040] like Figure 1~2 The present invention illustrates a silicon carbide smelting furnace capable of improving the first-grade silicon carbide yield, comprising a furnace bottom 1, an environmentally friendly sealed furnace wall 2 surrounded by refractory bricks and sealed with cement, the furnace bottom 1 being made of refractory bricks 11 including microchannels 111, the microchannels 111 extending from the top surface of the refractory bricks 11 to the bottom surface of the refractory bricks 11, the diameter of the microchannels 111 being 200 μm to 300 μm, and the density of the microchannels 111 in the refractory bricks 11 being 300 / cm 2 ~350pcs / cm 2 The smelting furnace further includes: an air duct 112 arranged at the lower layer of the furnace bottom 1 , the air duct 112 being composed of through holes laterally arranged on the refractory bricks 11 containing the microchannel 111 , and the air duct is connected to the microchannel 111 .

[0041] Specifically, Figure 3~4The height of the furnace bottom is 20 cm, which is paved with refractory bricks. A plurality of air ducts 112 are arranged horizontally below the furnace bottom. The diameter of each air duct 112 is 2 cm. The air ducts 112 below the furnace bottom are all connected to the lower flue gas channel 43. The lower flue gas channel 43 is connected to the flue gas main pipe through the lower flue gas pipe 42. The flue gas main pipe is connected to the tail gas recovery system 4. The air duct 112 is arranged below the furnace bottom 1. The air duct 112 is also made of refractory bricks. Specifically, the air duct is arranged horizontally on the refractory brick 11 provided with the microchannel 111. The air duct is connected to the microchannel 111, so that the flue gas in the microchannel 111 can enter the air duct 112.

[0042] Refractory bricks are laid around the furnace bottom 1 to form a furnace wall with a thickness of 20 cm. The refractory bricks are coated with cement to make the furnace wall an environmentally friendly sealed furnace wall 2. The main structure of the silicon carbide smelting furnace consists of the furnace bottom 1 and the furnace wall 2, forming a huge box-type furnace body. The size of the furnace body in the embodiment of the present application is length × width × height: 50m × 5m × 8m. The two sides of the longitudinal furnace wall are furnace heads 3, and the furnace heads 3 are installed with the heating electrode end of the silicon carbide smelting furnace, and the electrode end is connected to the transformer.

[0043] like Figure 1 At the top of the silicon carbide smelting furnace in the embodiment of the present application, a silicon carbide smelting fume collection hood 41 is provided, and the fume collection hood 41 is connected to the fume main pipe through the upper fume channel, and the fume main pipe is connected to the exhaust gas recovery system 4.

[0044] In the embodiment of the present application, the refractory bricks 11 used for laying the furnace bottom 1 are provided with microchannels 111 penetrating the brick body, the diameter of the microchannels is 200 μm to 300 μm, and the arrangement density of the microchannels is 300 to 350 per cm 2 The diameter and density of the microchannels satisfy the normal distribution. The diameter and density of the above microchannels are within ±2σ. For example, the diameter of 95.45% of the microchannels is distributed between 200μm and 300μm, and the density of 95.45% of the microchannels in the refractory brick is within 300 / cm 2 ~350 pieces / cm 2 .

[0045] In the embodiment of the present application, the tail gas recovery system 4 is a conventional carbonization furnace tail gas treatment system, which mainly includes a dust removal system and a desulfurization tower. Example

[0046] An embodiment of a furnace loading method for smelting silicon carbide using the smelting furnace of Example 1.

[0047] like Figure 2The schematic furnace loading area is divided into a heat preservation material area 55, a resistance material area 56, a first area 51, a second area 52, a third area 53, and a fourth area 54. The first area 51 is the furnace bottom area, the second area 52 is the furnace top area, the third area 53 is the area adjacent to the furnace wall, and the fourth area 54 is the other areas in the smelting furnace except the first area 51, the second area 52, the third area 53, the heat preservation material area 55, and the resistance material area 56;

[0048] The particle size of the silicon carbide smelting raw material laid in the first area 51 and the second area 52 is larger than that in the third area 53 and the fourth area 54. The particle size of the silicon carbide smelting raw material laid in the fourth area 54 is larger than that in the third area 53.

[0049] The particle size of the carbonaceous raw material in the silicon carbide smelting raw materials charged into the first area 51 is 3mm~4mm, and the particle size of the siliceous raw material is 6mm~10mm; the particle size of the carbonaceous raw material in the silicon carbide smelting raw materials charged into the second area 52 is 3mm~4mm, and the particle size of the siliceous raw material is 6mm~10mm; the particle size of the carbonaceous raw material in the silicon carbide smelting raw materials charged into the third area 53 is <2mm, and the particle size of the siliceous raw material is <1mm; the particle size of the carbonaceous raw material in the silicon carbide smelting raw materials charged into the fourth area 54 is 2mm~3mm, and the particle size of the siliceous raw material is 1mm~6mm. Among them, the particle size of the above-mentioned siliceous raw material and the particle size distribution of the siliceous raw material satisfy the normal distribution, and the above-mentioned particle size range is within ±2σ. For example, the particle size of the carbonaceous raw material in the silicon carbide smelting raw material loaded into the first area 51 is 3mm~4mm, and the particle size of the siliceous raw material is 6mm~10mm. In fact, 95.45% of the carbonaceous raw material has a particle size of 3mm~4mm, and 95.45% of the siliceous raw material has a particle size of 6mm~10mm.

[0050] The carbonaceous raw material is anthracite, and the siliceous raw material is silicon dioxide. The ratio of siliceous raw material to carbonaceous raw material is 1.18:1. In the siliceous raw material, the SiO2 content is ≥98%. In the carbonaceous raw material, the fixed carbon content is ≥80%, and the ash content is 3% to 10%.

[0051] The specific furnace loading process is:

[0052] Step 1:

[0053] First, lay the insulation material with a height of 40cm and a particle size of 3mm-5mm under the furnace body, and then continue to lay the insulation material area material, the first area material, and the third area material on top of the laid insulation material, among which:

[0054] The insulation material area is the area with a thickness of 40 cm from the furnace wall to the furnace, that is, the thickness of the insulation material laid in the insulation material area is 40 m.

[0055] Step 2: After the insulation material under the furnace body is laid, start laying the materials in the first area, the insulation material area materials at the same height as the materials in the first area, and the materials in the third area, as follows:

[0056] The insulation material area is the area with a thickness of 40 cm from the furnace wall to the furnace, that is, the thickness of the insulation material laid in the insulation material area is 40 m.

[0057] The third area is from the insulation material area located on the furnace wall to the area with a thickness of 50 cm in the furnace, that is, the material thickness laid in the third area is 50 m, the particle size of the carbonaceous raw material laid in the third area is less than 2 mm, and the particle size of the siliceous raw material is less than 1 mm;

[0058] The first area is located in the middle of the third area in the furnace. The laying starts from above the insulation material below the furnace body. The height of the laying material in the first area is 1m. The particle size of the carbonaceous raw material laid in the first area is 3mm~4mm, and the particle size of the siliceous raw material is 6mm~10mm.

[0059] Step 3: After the first area is paved, continue to pave the insulation area, the third area and the fourth area. The paving method of the insulation area and the third area is the same as step 2, as follows:

[0060] The insulation material area is the area with a thickness of 40 cm from the furnace wall to the furnace, that is, the thickness of the insulation material laid in the insulation material area is 40 m.

[0061] The third area is from the insulation material area located on the furnace wall to the area with a thickness of 50 cm in the furnace, that is, the material thickness laid in the third area is 50 m, the particle size of the carbonaceous raw material laid in the third area is less than 2 mm, and the particle size of the siliceous raw material is less than 1 mm;

[0062] The fourth area is located in the middle of the third area in the furnace, with a laying height of 1.5m starting from above the materials in the first area. The particle size of the carbonaceous raw materials laid in the fourth area is 2mm-3mm, and the particle size of the siliceous raw materials is 1mm-6mm.

[0063] Step 4: After step 3 is completed, continue to lay the insulation material area and the third area, the fourth area and the resistance material area on top of the material laid in step 3. The width of the resistance material is 40cm and the thickness is 60cm. The laying method of the insulation material area, the third area and the fourth area is the same as step 3, as follows:

[0064] The insulation material area is the area with a thickness of 40cm from the furnace wall to the furnace, that is, the thickness of the insulation material laid in the insulation material area is 40m;

[0065] The third area is from the insulation material area located on the furnace wall to the area with a thickness of 50 cm in the furnace, that is, the material thickness laid in the third area is 50 m, the particle size of the carbonaceous raw material laid in the third area is less than 2 mm, and the particle size of the siliceous raw material is less than 1 mm;

[0066] The fourth area is located in the middle of the third area in the furnace, and the laying height is 60 cm from the top of the material in the fourth area in step 3. The particle size of the carbonaceous raw material laid in the fourth area is 2 mm to 3 mm, and the particle size of the siliceous raw material is 1 mm to 6 mm.

[0067] The resistor material laid in the resistor material area is located in the center of the furnace body, crosses the smelting furnace horizontally, and is connected to the electrodes at both ends of the smelting furnace. The resistor material is graphite resistor material, with a laying width of 40cm and a thickness of 60cm.

[0068] Step 5: At the same time, continue to lay the insulation material area, the third area, and the fourth area materials on top of the materials laid in step 4, with a laying height of 90 cm. Specifically:

[0069] The insulation material area is the area with a thickness of 40cm from the furnace wall to the furnace, that is, the thickness of the insulation material laid in the insulation material area is 40m;

[0070] The third area is from the insulation material area located on the furnace wall to the area with a thickness of 50 cm in the furnace, that is, the material thickness laid in the third area is 50 m, the particle size of the carbonaceous raw material laid in the third area is less than 2 mm, and the particle size of the siliceous raw material is less than 1 mm;

[0071] The fourth area is located in the middle of the third area in the furnace. The laying height is 90 cm from the materials in the fourth area and the resistor material area in step four. The particle size of the carbonaceous raw material laid in the fourth area is 2mm~3mm, and the particle size of the siliceous raw material is 1mm~6mm.

[0072] Step 6: At the same time, continue to lay the insulation material area, the third area, and the second area materials on top of the materials laid in step 5, with a laying height of 1m, specifically:

[0073] The insulation material area is the area with a thickness of 40cm from the furnace wall to the furnace, that is, the thickness of the insulation material laid in the insulation material area is 40m;

[0074] The third area is from the insulation material area located on the furnace wall to the area with a thickness of 50 cm in the furnace, that is, the material thickness laid in the third area is 50 m, the particle size of the carbonaceous raw material laid in the third area is less than 2 mm, and the particle size of the siliceous raw material is less than 1 mm;

[0075] The second area is located above the third and fourth areas in the furnace. The laying height is 1m starting from the materials in the third and fourth areas in step five. The particle size of the carbonaceous raw materials laid in the second area is 3mm to 4mm, and the particle size of the siliceous raw materials is 6mm to 10mm.

[0076] Step 7: Continue to lay insulation material with a height of 40 cm on the insulation material area, the second area, and the third area laid in step 6.

[0077] In the above steps 1 to 7, the materials laid in the first area, the second area, the third area and the fourth area are materials obtained by mixing silicon raw materials and carbon raw materials in a mass ratio of 1.18:1.

[0078] After the furnace is loaded, power is turned on for smelting. The smelting process is as follows: the power of the power transmission transformer in the time period from 0 to 30.6 hours is 51000KVA, and the power of the power transmission transformer in the time period from 30.6 to 34 hours is set to 34000KVA. After the smelting is completed, it is cooled for 3 days and then taken out of the furnace to obtain silicon carbide.

[0079] After coming out of the furnace: first-grade SiC ≥98.5%, 803.93 tons of first-grade products; second-grade SiC: ≥90%, 447.57 tons of second-grade products; third-grade SiC: 60%~70%, 209.56 tons of third-grade products; the first-grade rate of silicon carbide is 55%.

[0080] Comparative Example 1

[0081] The silicon carbide smelting furnace used in Comparative Example 1 is a closed smelting furnace. The structure of the silicon carbide smelting furnace includes a furnace bottom 1, an environmentally friendly sealed furnace wall 2 surrounded by refractory bricks and sealed with cement above the furnace bottom, the furnace bottom is paved with conventional silicon carbide smelting furnace refractory bricks, and there is no ventilation channel at the furnace bottom.

[0082] Specifically, the height of the furnace bottom is 20 cm, which is paved with refractory bricks for ordinary silicon carbide smelting furnaces. Refractory bricks are laid around the furnace bottom to form a furnace wall with a thickness of 20 cm. The refractory bricks are coated with cement to make the furnace wall a sealed furnace wall. The main structure of the silicon carbide smelting furnace consists of a furnace bottom and a furnace wall, forming a huge box-type furnace body. The size of the furnace body in the embodiment of the present application is length × width × height: 50m × 5m × 8m. The two sides of the longitudinal furnace wall are furnace heads, and the furnace heads are equipped with heating electrode ends of the silicon carbide smelting furnace, and the electrode ends are connected to the transformer.

[0083] The top of the silicon carbide smelting furnace is provided with a silicon carbide smelting fume collection hood, which is connected to the fume main pipe through the upper fume channel, and the fume main pipe is connected to the tail gas recovery system 4. The silicon carbide smelting furnace of the comparative example is an environmentally friendly sealed silicon carbide smelting furnace. The tail gas recovery system 4 is a conventional carbide furnace tail gas treatment system, which mainly includes a dust removal system and a desulfurization tower.

[0084] like Figure 6 The conventional furnace loading area is also divided into an insulation material area, a resistance material area, and a reaction material area. The carbonaceous raw material laid in the reaction material area is anthracite, and the siliceous raw material is silicon dioxide. The particle size of the carbonaceous raw material in the reaction material area is 2mm-3mm, and the particle size of the siliceous raw material is 1mm-6mm. The particle size of the carbonaceous raw material and the particle size of the siliceous raw material meet the normal distribution. The above particle size range is within ±2σ, that is, 95.45% of the carbonaceous raw material has a particle size of 2mm-3mm, and 95.45% of the siliceous raw material has a particle size of 1mm-6mm. The ratio of siliceous raw material to carbonaceous raw material is 1.18:1. In the siliceous raw material, the SiO2 content is ≥98%. In the carbonaceous raw material, the fixed carbon content is ﹥80%, and the ash content is 3%-10%.

[0085] After the furnace is loaded, power is turned on for smelting. The smelting process is as follows: the power of the power transmission transformer in the time period from 0 to 30.6 hours is 51000KVA, and the power of the power transmission transformer in the time period from 30.6 to 34 hours is set to 34000KVA. After the smelting is completed, it is cooled for 3 days and then taken out of the furnace to obtain silicon carbide.

[0086] First-grade SiC≥98.5%, 700.22 tons of first-grade; second-grade SiC: ≥90%, 518.07 tons of second-grade; third-grade SiC: 60%~70%, 242.84 tons of third-grade; the first-grade rate of silicon carbide is 48%.

[0087] Through the above-mentioned Example 2 and Comparative Example 1 and Figure 5 and Figure 6 It can be found that the present invention improves the structure and materials of the furnace bottom 1 of the existing environmentally friendly sealed furnace. The furnace bottom 1 is paved with refractory bricks with microchannels 111, and the lower layer of the refractory bricks 111 is designed with an air guide 112 connected to the tail gas recovery system. Various gas phase side reaction products generated by the reaction during the silicon carbide smelting process and various harmful metals and metal oxides gasified at high temperature can be discharged from the microchannels at the bottom of the furnace, enter the tail gas recovery system through the air guide, and are discharged after purification. When loading the furnace, the bottom reaction zone area is increased, thereby expanding the superior product reaction zone.

[0088] like Figure 6 In the prior art, the particle sizes of the charge in each part of the silicon carbide furnace are consistent, which is not conducive to the permeability of the charge when used in a sealed smelting furnace, and the output rate of high-quality products is low. Figure 5In the present invention, materials of different particle sizes are laid at different cross-sectional positions in the furnace, and large-particle materials are laid in the furnace bottom and furnace top areas, so that a gas discharge channel can be formed between the bottom materials, ensuring that harmful gases can be discharged smoothly through the microchannels of the refractory brick layer at the bottom of the furnace. Small-particle materials are laid near the furnace wall, so that the harmful gases flowing in this direction are blocked from penetrating and are forced to be discharged upward or downward into the tail gas collection system. This technology significantly improves the air permeability of the sealed smelting furnace, reduces the impurity content of the product, and increases the first-grade rate of the product. At the same time, it can also ensure the directional collection of harmful gases and prevent them from being discharged into the atmosphere.

[0089] Through the application of the present invention, the first-grade rate of silicon carbide products is increased from 48% to 55%.

[0090] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for charging a smelting furnace capable of improving the first-grade rate of silicon carbide, characterized in that: A silicon carbide smelting furnace capable of improving the first-grade silicon carbide yield is used. The smelting furnace comprises a furnace bottom (1), and an environmentally friendly sealed furnace wall (2) formed on all sides above the furnace bottom by refractory bricks and sealed by cement coating. The furnace bottom (1) is made of refractory bricks (11) containing microchannels (111). The microchannels (111) penetrate from the top surface of the refractory bricks (11) to the bottom surface of the refractory bricks (11). The diameter of the microchannels (111) is 200 μm to 300 μm. The density of the microchannels (111) in the refractory bricks (11) is 300 / cm. 2 ~350pcs / cm 2 The smelting furnace further comprises: an air guide channel (112) arranged at the lower layer of the furnace bottom (1), the air guide channel (112) being composed of through holes arranged transversely on the refractory brick (11) containing the microchannel (111), and the air guide channel being in communication with the microchannel (111); In the furnace loading method, the furnace loading area is divided into a heat-insulating material area (55), a resistance material area (56), a first area (51), a second area (52), a third area (53), and a fourth area (54), wherein the first area (51) is a furnace bottom area, the second area (52) is a furnace top area, the third area (53) is an area adjacent to a furnace wall, and the fourth area (54) is other areas in the smelting furnace except the first area (51), the second area (52), the third area (53), the heat-insulating material area (55), and the resistance material area (56); The particle size of the silicon carbide smelting raw material laid in the first area (51) and the second area (52) is larger than the particle size of the silicon carbide smelting raw material laid in the third area (53) and the fourth area (54).

2. The furnace charging method according to claim 1, characterized in that: The particle size of the silicon carbide smelting raw material laid in the fourth area (54) is greater than the particle size of the silicon carbide smelting raw material laid in the third area (53).

3. The furnace charging method according to claim 2, characterized in that: The particle size of the carbonaceous raw material in the silicon carbide smelting raw material charged into the first zone (51) is 3mm to 4mm, and the particle size of the siliceous raw material is 6mm to 10mm; The second area (52) of the furnace is charged with silicon carbide smelting raw materials, the particle size of the carbonaceous raw material is 3mm ~ 4mm, the particle size of the siliceous raw material is 6mm ~ 10mm; The particle size of the carbonaceous raw material in the silicon carbide smelting raw material charged to the third zone (53) is less than 2 mm, and the particle size of the silicon raw material is less than 1 mm; The particle size of the carbonaceous raw material in the silicon carbide smelting raw material loaded into the furnace of the fourth zone (54) is 2 mm to 3 mm, and the particle size of the silicon raw material is 1 mm to 6 mm.

4. The furnace charging method according to claim 3, characterized in that: The carbonaceous raw material is anthracite, and the siliceous raw material is silicon dioxide.

5. The furnace charging method according to claim 3, characterized in that: The SiO2 content in the siliceous raw material is ≥98%.

6. The furnace charging method according to claim 3, characterized in that: The carbonaceous raw material has a fixed carbon content of >80% and an ash content of 3% to 10%.