Manufacturing method of device connection structure of silicon pillar array and device connection structure
By using a silicon column array manufacturing method in chip device connection, using alkaline wet etching and glass protective layer, the problems of low production efficiency and poor reliability in the prior art are solved, and high-deep vertical silicon micron columns are realized Processing reduces production costs and improves device connection stability.
Patent Information
- Application Number
- CN202311653726.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-04
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-12-04
AI Technical Summary
The existing chip device connection technology has problems such as low production efficiency, poor reliability, long time consumption and high production costs, especially in high-density packaging and micro-detailed devices.
Using the device connection structure manufacturing method of silicon column array, SiO2 mask is prepared by preliminary cleaning, pre-etching, thermal oxidation of silicon wafer wafers, and directional etching glue layer patterns are prepared by photolithography mechanism, and mixed with KOH and TMAH Alkaline wet etching is performed, surface impurities are removed and glass protective layer is poured to form a highly doped silicon column array.
It significantly reduces processing time and production costs, improves the stability and reliability of device connections, provides high-deep vertical silicon micro-pillars, providing new ideas and methods for high-density device connections.
Smart Images

Figure CN117672841B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of chip device interconnection, and in particular to a manufacturing method and a device connection structure of a silicon pillar array. Background Art
[0002] In the field of modern science and technology, the innovation of interconnection materials and processes within chips has become one of the most critical technical difficulties in the current development of high-end chips. The design of device connections and the manufacturing process methods are the key to achieving efficient, reliable and precise electronic device functions. There are four main types of existing packaging process chip interconnection technologies.
[0003] 1. Wire bonding: It uses metal wires with good conductivity (such as aluminum wires or gold wires) to connect the metal leads on the chip to the metal pins on the package substrate. 2. Flip chip bonding: In flip chip technology, the bare die and the substrate are no longer connected by wires. Instead, the chip is flipped and mounted upside down on the package substrate, and the connection is directly achieved through metal solder balls. 3. Hybrid bonding: First, through holes are formed by deep reactive ion etching or physical drilling, and copper is filled by electroplating. Then the surface is flattened by chemical mechanical grinding, and then the surface is activated by plasma to prepare for pre-bonding. After the upper and lower wafers are aligned, pre-bonding is completed, and after annealing, the diffusion of the copper through-hole bonding surface is further promoted to complete a good electrical connection. 4. Through-silicon via (TSV) bonding: TSV does not use traditional wiring methods to connect chips to chips, but vertically connects chips by drilling holes on the chip and filling them with conductive materials such as metal to accommodate electrodes. After making a wafer with TSVs, micro bumps are formed on its top and bottom through packaging, and then these bumps are connected.
[0004] However, the above-mentioned wire bonding still has some defects in high-density packaging and miniaturized devices. Wire bonding cannot meet the higher interconnection density requirements due to the limited line width. At the same time, due to its long electrical path, it is not suitable for newer devices that require high-speed operation. Flip-chip bonding requires strict process control and fine alignment operations to ensure bonding quality and reliability; at the same time, it is difficult to stack multiple chips, which is not conducive to storage products that require high density. Hybrid bonding is the focus of subsequent research and development because of its higher integration density and the ability to achieve both electrical connection and physical support, but this method is relatively complex and time-consuming, and has high production costs. The through-silicon via (TSV) bonding obtained by physical means has the disadvantages of low precision and low depth. Summary of the invention
[0005] The present invention provides a method for manufacturing a device connection structure of a silicon pillar array, aiming to solve the problems of low preparation efficiency, poor reliability, long time consumption, high production cost and poor quality of existing chip device connections.
[0006] An embodiment of the present invention provides a method for manufacturing a device connection structure of a silicon pillar array, the manufacturing method comprising the following steps:
[0007] S1. Silicon wafer preparation: preliminary cleaning and drying of silicon wafers;
[0008] S2. Etching crystal direction search: observe the target etching crystal direction through preliminary pre-etching in the center of the silicon wafer;
[0009] S3, mask preparation: preparing a SiO2 mask on the surface of the silicon wafer by thermal oxidation, and then preparing a directional etching glue layer pattern by a photolithography machine;
[0010] S4, alkaline wet etching: immersing the target silicon wafer in a mixture of KOH and TMAH for etching;
[0011] S5. Prepare a glass protective layer: remove surface impurities after etching and perform centrifugal washing and vacuum drying in sequence, and then pour molten glass on the surface to protect the silicon wafer.
[0012] Preferably, the step S1 specifically includes: washing the target silicon wafer (110) with deionized water, and then performing a vacuum drying process.
[0013] Preferably, the S2 specifically comprises the following steps:
[0014] S21, evenly spin-coating a 5 um adhesive layer on the surface of the silicon wafer, and then drying and curing the adhesive layer;
[0015] S22, placing the silicon wafer of S21 under a photolithography machine for alignment, and obtaining a square pre-etched opening at the center of the silicon wafer after exposure, development, washing, and drying;
[0016] S23, soaking the silicon wafer of S22 in a mixed etching solution of KOH and TMAH for 10 minutes, then taking it out and washing and drying it;
[0017] S24, placing the silicon wafer of S23 under a field emission scanning electron microscope to observe the etching surface, record the positioning angle θ, and mark the target crystal direction.
[0018] Preferably, in S22, the size of the square pre-etched opening pattern obtained after photolithography is 1×1 cm.
[0019] Preferably, in S23, after being in the mixed etching solution for 10 minutes, the following steps are further included:
[0020] The dried silicon wafer is placed under a microscope to observe the etching surface, find the crystal plane perpendicular to the surface and mark the crystal direction, and measure the target positioning angle θ.
[0021] Preferably, in S23, according to the mass ratio:
[0022] In the mixed etching solution, the content of KOH is 30wt%, the content of TMAH is 1wt%, the drying temperature is 50°C to 90°C, and the drying time is 1 to 2 hours.
[0023] Preferably, the S3 specifically includes the following steps:
[0024] S31, placing the silicon wafer with the crystal orientation marked thereon for oxidation in an ultrafast high temperature furnace;
[0025] S32, spin coating a 5 um adhesive layer on the surface of the silicon wafer in S31, and then drying and curing the adhesive layer;
[0026] S33, placing the silicon wafer in S32 under a photolithography machine and aligning it with a positioning mark line, and obtaining a pre-designed mask pattern after exposure, development, washing, and drying;
[0027] S34, removing excess SiO2 outside the mask area using a BOE solution.
[0028] Preferably, in S31, the oxidation temperature is 1100° C. and the heating time is 2 min.
[0029] Preferably, the S4 specifically comprises the following steps:
[0030] Use etching liquid to carve vertical silicon pillar arrays on the surface. Immerse the target silicon wafer with double-layer mask in the etching tank of KOH and TMAH solution. Control the temperature at 85℃. Use ultrasonic stirring and etching liquid circulation to ensure the uniformity of etching in each place. When the etching time is up, remove it and clean it.
[0031] Among them, the etching time is 20 minutes and the ambient temperature is 27°C.
[0032] In a second aspect, an embodiment of the present invention provides a device connection structure, wherein the device connection structure is manufactured by the above-mentioned method for manufacturing a device connection structure of a silicon pillar array.
[0033] Compared with the prior art, the invention has the beneficial effects of performing preliminary cleaning and drying on the silicon wafer; observing the target etching crystal direction by preliminary pre-etching the center of the silicon wafer; preparing a SiO2 mask on the surface of the silicon wafer by thermal oxidation, and then preparing a directional etching glue layer pattern by a photolithography machine; soaking the target silicon wafer in a mixture of KOH and TMAH for etching; removing surface impurities after etching and centrifugal washing and vacuum drying in sequence, and then pouring molten glass on its surface to protect the silicon wafer. In this way, the highly doped silicon column array is processed by wet etching, which greatly reduces the processing time compared with dry etching, and wet etching has the advantages of simple operation and low cost, which can effectively reduce the processing difficulty and production cost; at the same time, a high-depth vertical silicon micron column array is obtained, which provides a new idea and method for high-density device connection. The anisotropic etching of the silicon wafer in the KOH solution makes the side (111) basically not corroded, thereby obtaining a smooth and complete silicon micron column, which provides a more stable and reliable connection for subsequent device connection, and helps to improve the reliability and long-term stability of the device. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] The present invention will be described in detail below in conjunction with the accompanying drawings. The above and other aspects of the present invention will become clearer and easier to understand through the detailed description made in conjunction with the following drawings. In the accompanying drawings:
[0035] Figure 1 is a flow chart of a method for manufacturing a device connection structure of a silicon pillar array provided by an embodiment of the present invention;
[0036] Figure 2 is a schematic diagram of S1 provided in an embodiment of the present invention;
[0037] Figure 3 is a schematic diagram of S2 provided in an embodiment of the present invention;
[0038] Figure 4 is a top view of the silicon pillar array mask of the present invention;
[0039] Figure 5 It is a schematic diagram of S4 provided in an embodiment of the present invention.
[0040] In the figure: 101, silicon wafer; 201, pre-etching opening; 301, mask layer; 401, silicon pillar array. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0042] Combined with Figure 1-Figure 5 As shown, an embodiment of the present invention provides a method for manufacturing a device connection structure of a silicon pillar array, and the manufacturing method comprises the following steps:
[0043] S1. Silicon wafer preparation: preliminary cleaning and drying of silicon wafers.
[0044] Preferably, the step S1 specifically includes: washing the target silicon wafer (110) with deionized water, and then performing a vacuum drying process.
[0045] S2. Etching crystal direction search: Observe the target etching crystal direction through preliminary pre-etching in the center of the silicon wafer.
[0046] S3. Mask preparation: A SiO2 mask is prepared on the surface of the silicon wafer by thermal oxidation, and then a directional etching glue layer pattern is prepared by a photolithography machine.
[0047] S4, alkaline wet etching: immersing the target silicon wafer in a mixture of KOH and TMAH for etching.
[0048] Among them, TMAH, the full name of which is Tetramethylammonium hydroxide, is a common organic amine salt alkaline compound, which is widely used in the fields of semiconductors, optics, chemistry, etc. In this article, it is used as an etchant for silicon wafers.
[0049] S5. Prepare a glass protective layer: remove surface impurities after etching and perform centrifugal washing and vacuum drying in sequence, and then pour molten glass on the surface to protect the silicon wafer.
[0050] Specifically, the silicon wafer is preliminarily cleaned and dried; the target etching crystal direction is observed by preliminarily pre-etching the center of the silicon wafer; a SiO2 mask is prepared on the surface of the silicon wafer by thermal oxidation, and a directional etching glue layer pattern is prepared by a photolithography machine; the target silicon wafer is immersed in a mixture of KOH and TMAH for etching; the surface impurities after etching are removed and centrifugal washing and vacuum drying are performed in sequence, and then molten glass is poured on the surface to protect the silicon wafer. In this way, the highly doped silicon column array is processed by wet etching, which greatly reduces the processing time compared with dry etching, and wet etching has the advantages of simple operation and low cost, which can effectively reduce the processing difficulty and production cost; the anisotropic etching of the silicon wafer in the KOH solution makes the side (111) basically not corroded, thereby obtaining a smooth and complete silicon micron column, which provides a more stable and reliable connection for subsequent device connection, and helps to improve the reliability and long-term stability of the device. The mask pattern of the target silicon micron column is designed by a photolithography machine, and the silicon wafer is immersed in a mixed solution of KOH and TMAH. The difference in the etching rate of silicon in different crystal directions is used to make the etching solution continuously etch vertically toward the (1 1 0) plane without corroding the side, thereby obtaining a high-depth vertical silicon column, which provides a new processing method for high-density device connection to meet the growing functional and size requirements.
[0051] In this embodiment, S2 specifically includes the following steps:
[0052] S21, evenly spin-coating a 5 um adhesive layer on the surface of the silicon wafer, and then drying and curing the adhesive layer;
[0053] S22, placing the silicon wafer of S21 under a photolithography machine for alignment, and obtaining a square pre-etched opening at the center of the silicon wafer after exposure, development, washing, and drying;
[0054] S23, immersing the silicon wafer of S22 in a mixed etching solution of KOH and TMAH for 10 minutes, then taking it out and washing and drying it.
[0055] S24, placing the silicon wafer of S23 under a field emission scanning electron microscope to observe the etching surface, record the positioning angle θ, and mark the target crystal direction.
[0056] Preferably, in S22, the size of the square pre-etched opening pattern obtained after photolithography is 1×1 cm.
[0057] Preferably, in S23, after being in the mixed etching solution for 10 minutes, the following steps are further included:
[0058] The dried silicon wafer is placed under a microscope to observe the etching surface, find the crystal plane perpendicular to the surface and mark the crystal direction, and measure the target positioning angle θ.
[0059] Preferably, in S23, according to the mass ratio:
[0060] In the mixed etching solution, the content of KOH is 30wt%, the content of TMAH is 1wt%, the drying temperature is 50°C to 90°C, and the drying time is 1 to 2 hours.
[0061] Specifically, the target etching crystal direction is observed by preliminary pre-etching the center of the silicon wafer. A thin and uniform layer of glue is spin-coated on the surface of the cleaned and dried silicon wafer. After a period of drying to solidify the surface glue layer, the silicon wafer is placed under a photolithography machine and exposed to a square area of 1x1cm in the center. Then, the uncured photoresist is dissolved with a developer to remove part of the photoresist in the exposed area. Finally, after necessary drying and cleaning, a pre-etched silicon wafer with the glue layer of the center hole removed is obtained. Then, the silicon wafer is immersed in a mixed solution of KOH and TMAH for pre-etching for 10 minutes, and then the excess glue layer and impurities on the surface are removed with an organic solvent, and then it is taken out for cleaning and drying. The dried silicon wafer is placed under a microscope to observe the etching surface, find the (111) crystal plane perpendicular to the surface and mark the crystal direction, and measure the angle of the target positioning angle θ.
[0062] In this embodiment, S3 specifically includes the following steps:
[0063] S31, placing the silicon wafer with the crystal orientation marked thereon for oxidation in an ultrafast high temperature furnace;
[0064] S32, spin coating a 5 um adhesive layer on the surface of the silicon wafer in S31, and then drying and curing the adhesive layer;
[0065] S33, placing the silicon wafer in S32 under a photolithography machine and aligning it with a positioning mark line, and obtaining a pre-designed mask pattern after exposure, development, washing, and drying;
[0066] S34, removing excess SiO2 outside the mask area using a BOE solution.
[0067] Preferably, in S31, the oxidation temperature is 1100° C. and the heating time is 2 min.
[0068] Specifically, a silicon wafer with a marked crystal orientation is placed in a high-temperature furnace, oxygen is introduced for high-temperature oxidation, and a 5um SiO2 protective film is obtained on the surface of the silicon wafer. After cooling to room temperature, a 5um thick glue layer is evenly spin-coated on the target silicon wafer. After a period of drying and curing the surface glue layer, the silicon wafer is placed under a photolithography machine to align the marked crystal orientation, and the diamond-shaped area distributed around the ring designed in advance is exposed. Then, the uncured photoresist is dissolved with a developer, and part of the photoresist in the exposed area is removed. Finally, after necessary drying and cleaning, a (111) crystal orientation glue layer mask perpendicular to the surface (110) is obtained. Finally, the excess SiO2 outside the mask area is removed with a BOE solution. At this point, the mask pattern is prepared.
[0069] In this embodiment, S4 specifically includes the following steps:
[0070] Use etching liquid to carve vertical silicon pillar arrays on the surface. Immerse the target silicon wafer with double-layer mask in the etching tank of KOH and TMAH solution. Control the temperature at 85℃. Use ultrasonic stirring and etching liquid circulation to ensure the uniformity of etching in each place. When the etching time is up, remove it and clean it.
[0071] Among them, the etching time is 20 minutes and the ambient temperature is 27°C.
[0072] Specifically, an etching liquid is used to etch a vertical silicon column array on the surface, and the target silicon wafer with a double-layer mask is immersed in an etching tank of KOH and TMAH solution. The temperature is controlled to be constant at 85°C, and ultrasonic stirring and etching liquid circulation are continuously used to ensure the uniformity of etching in each place. After the etching time is up, the wafer is fished out and cleaned.
[0073] In this embodiment, in S5, the rotation speed of the centrifugal washing is 500-800 rpm, and the washing time is 30-40 min;
[0074] The vacuum drying process has a drying temperature of 60 to 80° C. and a drying time of 3 to 4 hours.
[0075] Specifically, the surface impurities are removed and a glass protective layer is prepared. The remaining glue layer and SiO2 on the surface of the silicon wafer are removed with an organic solvent and hydrofluoric acid, and then the wafer is washed with deionized water and centrifuged and vacuum dried in sequence, and finally the target diamond-shaped silicon micro-pillars distributed around the ring are obtained on the silicon wafer. Subsequently, molten glass is poured on the surface to protect the silicon wafer, and the two end faces are thinned to expose the surface silicon layer, so that the highly doped silicon micro-pillars can be used to directly connect the devices.
[0076] The silicon wafer is a (1 1 0)-plane N-type doped wafer with a geometric size of 4 inches, a thickness of 500um, and a resistivity of 5-10Ω·cm.
[0077] In this embodiment, the specific manufacturing process is as follows:
[0078] A clean and impurity-free silicon wafer 101 is obtained by performing preliminary cleaning and drying treatment on the silicon wafer 101; the center of the silicon wafer 101 is preliminarily pre-etched to observe the target etching crystal direction to form a pre-etching port 201, and a SiO2 mask is prepared on the surface of the silicon wafer 101 by thermal oxidation, and then a plurality of mask layers 301 of directional etching glue layer patterns are prepared by a photolithography machine, and the mask layers 301 are a plurality of diamond patterns distributed in a ring around the circumference of the silicon wafer 101; an etched silicon column array 401 is obtained by performing alkaline wet etching on the silicon wafer surface outside the mask layer 301 area.
[0079] An embodiment of the present invention further provides a device connection structure of a silicon pillar array, and the device connection structure of a silicon pillar array is manufactured by the above-mentioned method for manufacturing the device connection structure of a silicon pillar array.
[0080] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, article or device. In the absence of more restrictions, an element defined by the sentence "includes a ..." does not exclude the existence of other identical elements in the process, article or device including the element.
[0081] The embodiments of the present invention are described above in conjunction with the accompanying drawings. What is disclosed is only the preferred embodiment of the present invention. However, the present invention is not limited to the above-mentioned specific implementation manner. The above-mentioned specific implementation manner is only illustrative rather than restrictive. Under the enlightenment of the present invention, ordinary technicians in this field can also make many forms and equivalent changes without departing from the scope of protection of the purpose of the present invention and the claims, all of which are within the protection of the present invention.
Claims
1. A method for manufacturing a device connection structure of a silicon pillar array, It is characterized in that The manufacturing method comprises the following steps: S1. Silicon wafer preparation: preliminary cleaning and drying of silicon wafers; S2, etching crystal direction search: observing the target etching crystal direction by preliminary pre-etching the center of the silicon wafer; The S2 specifically includes the following steps: S21, evenly spin-coating a 5 um adhesive layer on the surface of the silicon wafer, and then drying and curing the adhesive layer; S22, placing the silicon wafer of S21 under a photolithography machine for alignment, and obtaining a square pre-etched opening at the center of the silicon wafer after exposure, development, washing, and drying; S23, soaking the silicon wafer of S22 in a mixed etching solution of KOH and TMAH for 10 minutes, then taking it out and washing and drying it; S24, placing the silicon wafer of S23 under a field emission scanning electron microscope to observe the etching surface, record the positioning angle θ, and mark the target crystal direction; S3, mask preparation: SiO2 is prepared on the surface of the silicon wafer by thermal oxidation. 2 mask, and then use a photolithography machine to prepare a directional etching glue layer pattern; The silicon wafer with the crystal orientation marked is placed in a high-temperature furnace and oxygen is introduced for high-temperature oxidation to obtain a 5 μm thick SiO layer on the surface of the silicon wafer. 2 After cooling to room temperature, a 5um thick glue layer is evenly spin-coated on the target silicon wafer. After a period of drying and curing the surface glue layer, the silicon wafer is placed under the photolithography machine to align the marked crystal orientation, and the diamond-shaped area distributed around the ring designed in advance is exposed. Then, the uncured photoresist is dissolved with a developer to remove part of the photoresist in the exposed area. Finally, after drying and cleaning, a crystal orientation glue layer mask perpendicular to the surface is obtained; BOE solution is used to remove excess SiO outside the mask area. 2 , the mask pattern is prepared; S4, alkaline wet etching: immersing the target silicon wafer in a mixture of KOH and TMAH for etching; S5. Prepare a glass protective layer: remove surface impurities after etching and perform centrifugal washing and vacuum drying in sequence, and then pour molten glass on the surface to protect the silicon wafer.
2. The method for manufacturing the device connection structure of the silicon pillar array according to claim 1, It is characterized in that The S1 specifically includes: washing the silicon wafer with deionized water, and then performing a vacuum drying process.
3. The method for manufacturing the device connection structure of the silicon pillar array according to claim 1, It is characterized in that In the above S22, the size of the square pre-etched opening pattern obtained after photolithography is 1×1 cm.
4. The method for manufacturing the device connection structure of the silicon pillar array according to claim 1, It is characterized in that In the S23, after being in the mixed etching solution for 10 minutes, the following steps are also included: The dried silicon wafer is placed under a microscope to observe the etching surface, find the crystal plane perpendicular to the surface and mark the crystal direction, and measure the target positioning angle θ.
5. The method for manufacturing the device connection structure of the silicon pillar array according to claim 1, It is characterized in that In said S23, according to the mass ratio: In the mixed etching solution, the content of KOH is 30wt%, the content of TMAH is 1wt%, the drying temperature is 50°C to 90°C, and the drying time is 1 to 2 hours.
6. The method for manufacturing the device connection structure of the silicon pillar array according to claim 1, It is characterized in that In S3, the oxidation temperature is 1100° C. and the heating time is 2 minutes.
7. The method for manufacturing the device connection structure of the silicon pillar array according to claim 1, It is characterized in that The S4 specifically comprises the following steps: Use etching liquid to carve vertical silicon pillar arrays on the surface. Immerse the target silicon wafer with double-layer mask in the etching tank of KOH and TMAH solution. Control the temperature at 85℃. Use ultrasonic stirring and etching liquid circulation to ensure the uniformity of etching in each place. When the etching time is up, remove it and clean it. Wherein, the etching time is 20 minutes and the ambient temperature is 27°C.
8. A device connection structure, It is characterized in that The device connection structure is manufactured by the method for manufacturing a device connection structure of a silicon pillar array according to any one of claims 1 to 7.