Highly dispersed nano zinc oxide for rubber and preparation method thereof

Through the preparation of composite zinc oxide and the modification of nano-zinc oxide, combined with the cyanation of graphene oxide and silica and the addition of nano-short fibers, the problem of nano-zinc oxide agglomeration in rubber is solved and high dispersion is achieved and good mechanical properties, improving the overall performance of rubber.

CN117683347BActive Publication Date: 2024-10-01JIANGSU ATE DONGTAI NEW MATERIALS TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311558539.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-22
Publication Date
2024-10-01
Estimated Expiration
2043-11-22

AI Technical Summary

Technical Problem

Nano-zinc oxide is prone to agglomeration during rubber preparation, resulting in poor dispersion and hindering its widespread application.

Method used

The preparation method of composite zinc oxide A and composite zinc oxide B is used, combined with the cyanation modification of graphene oxide and silica, and the addition of short nanofibers, and through steps such as ultrasonic dispersion and magnetic stirring, a highly dispersed Nano-zinc oxide inhibits its agglomeration and improves dispersion and mechanical properties.

Benefits of technology

It achieves high dispersion and low aggregation of nano-zinc oxide in rubber, while improving the comprehensive mechanical properties and dispersion of rubber, ensuring the effective performance of nano-zinc oxide as an accelerator and vulcanizing agent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004561796180000081
    Figure BDA0004561796180000081
  • Figure BDA0004561796180000091
    Figure BDA0004561796180000091
Patent Text Reader

Abstract

The invention relates to the technical field of rubber preparation, and discloses a highly dispersed nano zinc oxide for rubber and a preparation method thereof; the invention uses a zinc oxide active agent as a main component to prepare a zinc oxide active substance, and uses it as an active component of the rubber to participate in the reaction. The invention selects nano zinc oxide with a smaller particle size, and uses graphene oxide and silicon dioxide to hybridize it respectively: firstly, by using the silicon dioxide surface deposition method, the problem of easy agglomeration of nano zinc oxide can be improved; secondly, because graphene oxide has excellent chemical inertness, high mechanical strength, high optical transparency and other good properties, it is used as another main component of hybrid nano zinc oxide for reaction, and graphene oxide is used as a reinforcing phase of nano zinc dioxide to effectively improve its interface bonding strength; finally, the invention designs and synthesizes a short-cut cellulose, which improves its crosslinking density and enhances the mechanical properties of the rubber at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber preparation, in particular to highly dispersed nano zinc oxide for rubber and a preparation method thereof. Background Art

[0002] With the widespread use of rubber products in life, enhancing their comprehensive performance has become an important topic. Common rubber products often use zinc oxide as a vulcanizer, accelerator and activator for traditional rubber products, playing an important role in the preparation and production of rubber. During the mixing process with the rubber, zinc oxide is prone to dispersion and gelation of the rubber.

[0003] Since nano zinc oxide has a smaller particle size, larger specific surface area and higher activity, in order to obtain a more environmentally friendly preparation process, nano zinc oxide is gradually used to replace ordinary zinc oxide, which increases the reaction contact sites while improving the vulcanization activity. At the same time, nano zinc oxide is very easy to agglomerate, which seriously hinders its widespread application.

[0004] In order to solve the above problems, it is necessary to design and synthesize a nano zinc oxide that has a promoting and activating effect while reducing the tendency to agglomerate and being highly dispersed. Summary of the invention

[0005] The object of the present invention is to provide a highly dispersed nano zinc oxide for rubber and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A method for preparing highly dispersed nano zinc oxide for rubber has the following steps:

[0008] S1: Preparation of composite zinc oxide A:

[0009] (1) Mix zinc acetate dihydrate and anhydrous ethanol, heat to 80-90° C., and stir magnetically for 30-40 minutes to obtain a mixed solution;

[0010] (2) lithium hydroxide dihydrate and graphene oxide are ultrasonically dispersed in anhydrous ethanol and then mixed evenly, and then dropped into the prepared mixed solution, reacted at 80-90° C. for 30-40 min, cooled to 20-30° C., added with n-hexane, and allowed to settle at 4-6° C. for 12-14 h, washed, vacuum dried at 60-70° C. for 24-30 h, and ground to obtain composite zinc oxide A;

[0011] S2: Preparation of composite zinc oxide B:

[0012] (1) SiO2, ammonia water and deionized water are mixed, and after ultrasonic treatment, tricyanopropyltriethoxysilane is added dropwise, the temperature is raised to 50-60°C, stirred for 24-30 hours, vacuum filtered, and dried overnight to obtain an intermediate product;

[0013] (2) mixing the prepared intermediate product, zinc acetate and ethylene glycol, ultrasonically dispersing, adding ammonia water, heating to 60-70° C., reacting for 24-30 hours, centrifuging and grinding to obtain composite zinc oxide B;

[0014] S3: Preparation of short fiber composites:

[0015] Take aramid nano short fibers and dispersant, put them into a grinder and grind them for 20 to 30 minutes, take epoxy resin, stir at high speed for 20 to 30 minutes to obtain a short fiber composite;

[0016] S4: taking the prepared composite zinc oxide A, composite zinc oxide B, and short fiber composite, and blending them in a weight ratio of (1-1.5):(1-2):1 to obtain a highly dispersed nano zinc oxide for rubber.

[0017] More optimally, in S1(1), the ingredients are: by weight, 0.5-1 parts of zinc acetate dihydrate and 50-60 parts of anhydrous ethanol.

[0018] More optimally, in S1(2), the ingredients are: 0.2-0.4 parts of lithium hydroxide dihydrate and 0.06-0.1 parts of graphene oxide, by weight.

[0019] More optimally, in S1(2), the volume ratio of n-hexane to the reaction solution is (2-2.5):1.

[0020] More optimally, in S2, the ingredients are: 4 to 8 parts of silicon dioxide, 6 to 10 parts of ammonia water, 30 to 40 parts of deionized water, 2 to 3 parts of tricyanopropyltriethoxysilane, 8 to 14 parts of zinc acetate, and 5 to 10 parts of ammonia water.

[0021] More optimally, in S3, the dispersant is polyethylene oxide and the stirring speed is 1000 rad / min.

[0022] More optimally, in S3, the ingredients are: by weight, 100-150 parts of aramid nano short fibers, 5-10 parts of dispersant, and 1-2 parts of epoxy resin.

[0023] More optimally, the preparation steps of the rubber are: take styrene-butadiene rubber, high cis-1,2-butadiene rubber, accelerator, composite zinc oxide A, composite zinc oxide B, a blended product of a short fiber composite, microcrystalline wax, stearic acid, carbon black, and environmentally friendly oil, mix them to 150-160°C, then discharge the rubber, leave them for 4-5 hours, then add sulfur, accelerator, and anti-scorch agent, and after the reaction is completed, a highly dispersed nano zinc oxide rubber is prepared.

[0024] More optimally, in the rubber preparation step, the accelerator is NS and the anti-scorch agent is CTP.

[0025] More optimally, in the rubber preparation step, the ingredients are: in parts by weight, 40 to 50 parts of styrene-butadiene rubber, 60 to 70 parts of high cis-1,4-butadiene rubber, 1 to 2 parts of accelerator, 1 to 2 parts of composite zinc oxide A, 1 to 2 parts of composite zinc oxide B, 1 to 2 parts of short fiber composites, 1 to 2 parts of microcrystalline wax, 0.5 to 1.5 parts of stearic acid, 55 to 60 parts of carbon black, 14 to 20 parts of environmentally friendly oil, 1 to 2 parts of sulfur, and 1 to 2 parts of anti-scorch agent.

[0026] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0027] (1) The present invention designs and synthesizes a nano zinc dioxide prepared by hybrid modification of silicon dioxide, wherein silicon dioxide is cyanated by cyano groups, and cyano groups are introduced on the surface of silicon dioxide to prepare silicon dioxide with good adsorption performance and reinforcement effect. At the same time, the presence of cyano groups is conducive to the nucleation and growth of nano zinc oxide on its surface, inhibiting the overlapping growth between nano zinc oxide particles, thereby ensuring the dispersibility of the system;

[0028] (2) Graphene oxide is a new type of material with excellent performance. Adding it to nano zinc oxide as a reinforcing phase ensures the excellent performance of graphene oxide while enhancing its binding performance with other substances. Graphene oxide can play a good dispersing role. Using nano zinc dioxide after hybrid modification of graphene oxide as one of the additives for rubber products ensures the uniform distribution of nano zinc dioxide and enhances the performance of nano zinc dioxide as an accelerator and vulcanizer.

[0029] (3) The present invention designs and synthesizes a nano short fiber, which is used as an additive in the rubber preparation process, and works in synergy with nano zinc dioxide to ensure the dispersion of the nano short fiber in the rubber matrix and improve the comprehensive mechanical properties of the resin. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] A method for preparing highly dispersed nano zinc oxide for rubber includes the following chemicals:

[0032] Graphene oxide: Model: SY-rGO-S, Brand: SmartCmeta, Beijing Meiston Technology Development Co., Ltd., Silicon dioxide: Specification: 20nm, Nanjing Baoket New Materials Co., Ltd., Tricyanopropyltriethoxysilane: Model: 24801-88-5, Pand (Shanghai) International Trade Co., Ltd., Aramid nano short fiber: Item No.: SWTFL-0001, Length: 3mm, Dongguan Sovit Special Wire and Tape Co., Ltd., Polyethylene oxide: Model: 10, Zaozhuang Xinghao New Materials Co., Ltd., Epoxy resin: E44, model: 6101, Langfang Ouyate Anti-corrosion Materials Co., Ltd., styrene-butadiene rubber: Brand: Sinopec, item number: SBR1502, Guangdong Housheng New Materials Co., Ltd., high-cis-butadiene rubber: model: BR9000, Shanghai Jinju International Trade Co., Ltd., accelerator: model: 95-31-8, Nantong Runfeng Chemical Co., Ltd., microcrystalline wax: model: 80#, Zhonghe Chemical (Shandong) Co., Ltd., anti-scorch agent: model: CTP (PVI) -01, Jinan Zhiheng Zhiyuan Chemical Technology Co., Ltd.

[0033] The following parts are by mass:

[0034] Embodiment 1:

[0035] S1: Mix 0.1 parts of zinc acetate dihydrate and 50 parts of anhydrous ethanol, heat to 80°C, and stir magnetically for 30 minutes to obtain a mixed solution;

[0036] S2: Take 0.2 parts of lithium hydroxide dihydrate and 0.06 parts of graphene oxide, disperse them in anhydrous ethanol by ultrasonic and mix them evenly, add them dropwise into the prepared mixed solution, react at 80°C for 30 minutes, cool to 20°C, add n-hexane, keep the system temperature at 4°C and let settle for 12 hours, wash, dry in vacuum at 60°C for 24 hours, grind to obtain composite zinc oxide A;

[0037] S3: 4 parts of silicon dioxide, 8 parts of ammonia water and deionized water were mixed, and 2 parts of tricyanopropyltriethoxysilane were added dropwise after ultrasonic treatment for 10 minutes. The mixture was heated to 50°C, stirred for 24 hours, vacuum filtered and dried overnight to obtain an intermediate product.

[0038] S4: Take the prepared intermediate product, 10 parts of zinc acetate, and 20 parts of ethylene glycol, mix them, ultrasonically disperse them for 10 minutes, add 5 parts of ammonia water, heat to 60°C, react for 24 hours, and centrifuge for 5 minutes to obtain composite zinc oxide B;

[0039] S5: 100 parts of aramid nano short fibers and 10 parts of dispersant were put into a grinder and crushed for 20 minutes, and 1 part of epoxy resin was taken and stirred at a speed of 1000 rad / min for 20 minutes to obtain a short fiber composite;

[0040] S6: Take 40 parts of styrene-butadiene rubber, 60 parts of high cis-1,4-butadiene rubber, 1 part of accelerator, 1.5 parts of composite zinc oxide A, 2 parts of composite zinc oxide B, 1 part of short fiber compound, 1.5 parts of microcrystalline wax, 1 part of stearic acid, 55 parts of carbon black, and 18 parts of environmentally friendly oil, mix them to 150°C and then discharge the glue. After standing for 4 hours, add 1 part of sulfur and 1 part of anti-scorch agent. After the reaction is completed, highly dispersed nano zinc oxide rubber is prepared.

[0041] Embodiment 2:

[0042] S1: Mix 0.1 parts of zinc acetate dihydrate and 50 parts of anhydrous ethanol, heat to 80°C, and stir magnetically for 30 minutes to obtain a mixed solution;

[0043] S2: Take 0.05 parts of lithium hydroxide dihydrate and 0.06 parts of graphene oxide, disperse them in anhydrous ethanol by ultrasonic and mix them evenly, add them dropwise into the prepared mixed solution, react at 80°C for 30 minutes, cool to 20°C, add n-hexane, keep the system temperature at 4°C and let settle for 12 hours, wash, dry in vacuum at 60°C for 24 hours, grind to obtain composite zinc oxide A;

[0044] S3: 4 parts of silicon dioxide, 8 parts of ammonia water and deionized water were mixed, and 2 parts of tricyanopropyltriethoxysilane were added dropwise after ultrasonic treatment for 10 minutes. The mixture was heated to 50°C, stirred for 24 hours, vacuum filtered and dried overnight to obtain an intermediate product.

[0045] S4: Take the prepared intermediate product, 10 parts of zinc acetate, and 20 parts of ethylene glycol, mix them, ultrasonically disperse them for 10 minutes, add 5 parts of ammonia water, heat to 60°C, react for 24 hours, and centrifuge for 5 minutes to obtain composite zinc oxide B;

[0046] S5: 100 parts of aramid nano short fibers and 10 parts of dispersant were put into a grinder and crushed for 20 minutes, and 1 part of epoxy resin was taken and stirred at a speed of 1000 rad / min for 20 minutes to obtain a short fiber composite;

[0047] S6: Take 40 parts of styrene-butadiene rubber, 60 parts of high cis-1,4-butadiene rubber, 1 part of accelerator, 1.5 parts of composite zinc oxide A, 2 parts of composite zinc oxide B, 1 part of short fiber compound, 1.5 parts of microcrystalline wax, 1 part of stearic acid, 55 parts of carbon black, and 18 parts of environmentally friendly oil, mix them to 150°C and then discharge the glue. After standing for 4 hours, add sulfur and 1 part of anti-scorch agent. After the reaction is completed, highly dispersed nano zinc oxide rubber is prepared.

[0048] Embodiment 3:

[0049] S1: Mix 0.1 parts of zinc acetate dihydrate and 50 parts of anhydrous ethanol, heat to 80°C, and stir magnetically for 30 minutes to obtain a mixed solution;

[0050] S2: Take 0.2 parts of lithium hydroxide dihydrate and 0.06 parts of graphene oxide, disperse them in anhydrous ethanol by ultrasonic and mix them evenly, add them dropwise into the prepared mixed solution, react at 80°C for 30 minutes, cool to 20°C, add n-hexane, keep the system temperature at 4°C and let settle for 12 hours, wash, dry in vacuum at 60°C for 24 hours, grind to obtain composite zinc oxide A;

[0051] S3: Mix 2 parts of silicon dioxide, 8 parts of ammonia water and deionized water, ultrasonically treat for 10 minutes, add 2 parts of tricyanopropyltriethoxysilane dropwise, heat to 50°C, stir for 24 hours, vacuum filter, and dry overnight to obtain an intermediate product;

[0052] S4: Take the prepared intermediate product, 10 parts of zinc acetate, and 20 parts of ethylene glycol, mix them, ultrasonically disperse them for 10 minutes, add 5 parts of ammonia water, heat to 60°C, react for 24 hours, and centrifuge for 5 minutes to obtain composite zinc oxide B;

[0053] S5: 100 parts of aramid nano short fibers and 10 parts of dispersant were put into a grinder and crushed for 20 minutes, and 1 part of epoxy resin was taken and stirred at a speed of 1000 rad / min for 20 minutes to obtain a short fiber composite;

[0054] S6: Take 40 parts of styrene-butadiene rubber, 60 parts of high cis-1,4-butadiene rubber, 1 part of accelerator, 1.5 parts of composite zinc oxide A, 2 parts of composite zinc oxide B, 1 part of short fiber compound, 1.5 parts of microcrystalline wax, 1 part of stearic acid, 55 parts of carbon black, and 18 parts of environmentally friendly oil, mix them to 150°C and then discharge the glue. After standing for 4 hours, add sulfur and 1 part of anti-scorch agent. After the reaction is completed, highly dispersed nano zinc oxide rubber is prepared.

[0055] Embodiment 4:

[0056] S1: Mix 0.1 parts of zinc acetate dihydrate and 50 parts of anhydrous ethanol, heat to 80°C, and stir magnetically for 30 minutes to obtain a mixed solution;

[0057] S2: Take 0.2 parts of lithium hydroxide dihydrate and 0.06 parts of graphene oxide, disperse them in anhydrous ethanol by ultrasonic and mix them evenly, add them dropwise into the prepared mixed solution, react at 80°C for 30 minutes, cool to 20°C, add n-hexane, keep the system temperature at 4°C and let settle for 12 hours, wash, dry in vacuum at 60°C for 24 hours, grind to obtain composite zinc oxide A;

[0058] S3: Mix 4 parts of silicon dioxide, 8 parts of ammonia water and deionized water, ultrasonically treat for 10 minutes, add 1 part of tricyanopropyltriethoxysilane dropwise, heat to 50°C, stir for 24 hours, vacuum filter, and dry overnight to obtain an intermediate product;

[0059] S4: Take the prepared intermediate product, 10 parts of zinc acetate, and 20 parts of ethylene glycol, mix them, ultrasonically disperse them for 10 minutes, add 5 parts of ammonia water, heat to 60°C, react for 24 hours, and centrifuge for 5 minutes to obtain composite zinc oxide B;

[0060] S5: 100 parts of aramid nano short fibers and 10 parts of dispersant were put into a grinder and crushed for 20 minutes, and 1 part of epoxy resin was taken and stirred at a speed of 1000 rad / min for 20 minutes to obtain a short fiber composite;

[0061] S6: Take 40 parts of styrene-butadiene rubber, 60 parts of high cis-1,4-butadiene rubber, 1 part of accelerator, 1.5 parts of composite zinc oxide A, 2 parts of composite zinc oxide B, 1 part of short fiber compound, 1.5 parts of microcrystalline wax, 1 part of stearic acid, 55 parts of carbon black, and 18 parts of environmentally friendly oil, mix them to 150°C and then discharge the glue. After standing for 4 hours, add 1 part of sulfur and 1 part of anti-scorch agent. After the reaction is completed, highly dispersed nano zinc oxide rubber is prepared.

[0062] Comparative Example 1: The addition of tricyanopropyltriethoxysilane was eliminated during the preparation of composite zinc oxide B, and the other conditions were kept the same as those in Example 1:

[0063] S1: Mix 0.1 parts of zinc acetate dihydrate and 50 parts of anhydrous ethanol, heat to 80°C, and stir magnetically for 30 minutes to obtain a mixed solution;

[0064] S2: Take 0.2 parts of lithium hydroxide dihydrate and 0.06 parts of graphene oxide, disperse them in anhydrous ethanol by ultrasonic and mix them evenly, add them dropwise into the prepared mixed solution, react at 80°C for 30 minutes, cool to 20°C, add n-hexane, keep the system temperature at 4°C and let settle for 12 hours, wash, dry in vacuum at 60°C for 24 hours, grind to obtain composite zinc oxide A;

[0065] S3: Mix 4 parts of silica, 8 parts of ammonia water and deionized water, treat with ultrasound for 10 minutes, vacuum filter, and dry overnight to obtain an intermediate product;

[0066] S4: Take the prepared intermediate product, 10 parts of zinc acetate, and 20 parts of ethylene glycol, mix them, ultrasonically disperse them for 10 minutes, add 5 parts of ammonia water, heat to 60°C, react for 24 hours, and centrifuge for 5 minutes to obtain composite zinc oxide B;

[0067] S5: 100 parts of aramid nano short fibers and 10 parts of dispersant were put into a grinder and crushed for 20 minutes, and 1 part of epoxy resin was taken and stirred at a speed of 1000 rad / min for 20 minutes to obtain a short fiber composite;

[0068] S6: Take 40 parts of styrene-butadiene rubber, 60 parts of high cis-1,4-butadiene rubber, 1 part of accelerator, 1.5 parts of composite zinc oxide A, 2 parts of composite zinc oxide B, 1 part of short fiber compound, 1.5 parts of microcrystalline wax, 1 part of stearic acid, 55 parts of carbon black, and 18 parts of environmentally friendly oil, mix them to 150°C and then discharge the glue. After standing for 4 hours, add 1 part of sulfur and 1 part of anti-scorch agent. After the reaction is completed, highly dispersed nano zinc oxide rubber is prepared.

[0069] Comparative Example 2: The preparation of composite zinc oxide A was omitted, and the other conditions were kept consistent with those of Example 1:

[0070] S1: Mix 4 parts of silicon dioxide, 8 parts of ammonia water and deionized water, ultrasonically treat for 10 minutes, add 2 parts of tricyanopropyltriethoxysilane dropwise, heat to 50°C, stir for 24 hours, vacuum filter, and dry overnight to obtain an intermediate product;

[0071] S2: Take the prepared intermediate product, 10 parts of zinc acetate, and 20 parts of ethylene glycol, mix them, ultrasonically disperse them for 10 minutes, add 5 parts of ammonia water, heat to 60°C, react for 24 hours, and centrifuge for 5 minutes to obtain composite zinc oxide;

[0072] S3: 100 parts of aramid nano short fibers and 10 parts of dispersant were put into a grinder and crushed for 20 minutes, and 1 part of epoxy resin was taken and stirred at a speed of 1000 rad / min for 20 minutes to obtain a short fiber composite;

[0073] S4: Take 40 parts of styrene-butadiene rubber, 60 parts of high cis-1,4-butadiene rubber, 1 part of accelerator, 2 parts of composite zinc oxide, 1 part of short fiber compound, 1.5 parts of microcrystalline wax, 1 part of stearic acid, 55 parts of carbon black, and 18 parts of environmentally friendly oil, mix them to 150°C and then discharge the glue. After standing for 4 hours, add 1 part of sulfur and 1 part of anti-scorch agent. After the reaction is completed, highly dispersed nano zinc oxide rubber is prepared.

[0074] Comparative Example 3: The preparation step of composite zinc oxide B was eliminated, and the other conditions were kept consistent with those in Example 1:

[0075] S1: Mix 0.1 parts of zinc acetate dihydrate and 50 parts of anhydrous ethanol, heat to 80°C, and stir magnetically for 30 minutes to obtain a mixed solution;

[0076] S2: Take 0.2 parts of lithium hydroxide dihydrate and 0.06 parts of graphene oxide, disperse them in anhydrous ethanol by ultrasonic and mix them evenly, add them dropwise into the prepared mixed solution, react at 80°C for 30 minutes, cool to 20°C, add n-hexane, keep the system temperature at 4°C and let settle for 12 hours, wash, dry in vacuum at 60°C for 24 hours, grind to obtain composite zinc oxide;

[0077] S3: 100 parts of aramid nano short fibers and 10 parts of dispersant were put into a grinder and crushed for 20 minutes, and 1 part of epoxy resin was taken and stirred at a speed of 1000 rad / min for 20 minutes to obtain a short fiber composite;

[0078] S4: 40 parts of styrene-butadiene rubber, 60 parts of high cis-1,4-butadiene rubber, 1 part of accelerator, 1.5 parts of composite zinc oxide, 1 part of short fiber compound, 1.5 parts of microcrystalline wax, 1 part of stearic acid, 55 parts of carbon black and 18 parts of environmentally friendly oil are mixed to 150°C and then discharged. After standing for 4 hours, 1 part of sulfur and 1 part of anti-scorch agent are added. After the reaction is completed, highly dispersed nano zinc oxide rubber is prepared.

[0079] Comparative Example 4: The preparation steps of composite zinc oxide A and composite zinc oxide B were eliminated, and the other conditions were kept the same as those in Example 1:

[0080] S1: Take 100 parts of aramid nano short fibers and 10 parts of dispersant, put them into a grinder and grind them for 20 minutes, take 1 part of epoxy resin, stir them at a speed of 1000 rad / min for 20 minutes to obtain a short fiber composite;

[0081] S2: Take 40 parts of styrene-butadiene rubber, 60 parts of high cis-1,4-butadiene rubber, 1 part of accelerator, 1.5 parts of composite zinc oxide A, 2 parts of composite zinc oxide B, 1 part of short fiber compound, 1.5 parts of microcrystalline wax, 1 part of stearic acid, 55 parts of carbon black, and 18 parts of environmentally friendly oil, mix them to 150°C and then discharge the glue. After standing for 4 hours, add 1 part of sulfur and 1 part of anti-scorch agent. After the reaction is completed, highly dispersed nano zinc oxide rubber is prepared.

[0082] Experiment: (1) The prepared composite zinc oxide A, composite zinc oxide B, and short fiber composite were blended with ethylene glycol at a weight ratio of 1:1:1, and the suspension was dropped onto a scanning electron microscope stage. After drying, it was observed using an electron microscope and the dispersion was recorded;

[0083] (2) The tensile properties of the prepared rubber product were tested according to the standard GB / T 528-2009. The obtained data are shown in the following table:

[0084] Table 1 Performance test data

[0085]

[0086]

[0087] Conclusion: By comparing the data in Table 1, it can be seen that the rubber product prepared according to Example 1 has better dispersibility, and still has good mechanical properties while maintaining its dispersibility. Adjusting the amount of each component will lead to a decrease in its performance. The ratio given in the present invention is the best ratio;

[0088] It can be seen from the comparative example that the presence of short fibers will improve the dispersion performance of the product, and the performance difference between graphene oxide and graphene will also affect the product. It is better to use graphene oxide as the raw material; the cyanation reaction of silica will obviously affect the subsequent reaction, and canceling the cyanation reaction may lead to uneven dispersion of nano zinc oxide and affect the performance; the steps of silica-modified nano zinc oxide and graphene-modified nano zinc oxide have a greater influence on the dispersion performance of the product, and at the same time will also affect its comprehensive performance.

[0089] In summary, the data show that the highly dispersed nano zinc oxide for rubber and the preparation method thereof provided by the present invention can prepare rubber with high dispersion and low agglomeration.

[0090] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing rubber from highly dispersed nano zinc oxide for rubber, characterized in that: Here are the steps: S1: Preparation of composite zinc oxide A: (1) Mix zinc acetate dihydrate and anhydrous ethanol, heat to 80-90° C., and stir magnetically for 30-40 minutes to obtain a mixed solution; wherein the mixed solution comprises: 0.5-1 parts of zinc acetate dihydrate and 50-60 parts of anhydrous ethanol, by weight; (2) lithium hydroxide dihydrate and graphene oxide are ultrasonically dispersed in anhydrous ethanol and then mixed evenly, and then added dropwise to the prepared mixed solution, reacted at 80-90° C. for 30-40 min, cooled to 20-30° C., added n-hexane, and allowed to settle at 4-6° C. for 12-14 h, washed, vacuum dried at 60-70° C. for 24-30 h, and ground to obtain composite zinc oxide A; the ingredients are: 0.2-0.4 parts of lithium hydroxide dihydrate and 0.06-0.1 parts of graphene oxide, in parts by weight; S2: Preparation of composite zinc oxide B: (1) SiO2, ammonia water and deionized water are mixed, and after ultrasonic treatment, (3-cyanopropyl)triethoxysilane is added dropwise, the temperature is raised to 50-60°C, stirred for 24-30 hours, vacuum filtered, and dried overnight to obtain an intermediate product; (2) taking the prepared intermediate product, zinc acetate, and ethylene glycol, mixing them, ultrasonically dispersing them, adding ammonia water, heating them to 60-70° C., reacting them for 24-30 hours, centrifuging them, and grinding them to obtain composite zinc oxide B; the components are as follows: 4-8 parts of silicon dioxide, 6-10 parts of ammonia water, 30-40 parts of deionized water, 2-3 parts of (3-cyanopropyl)triethoxysilane, 8-14 parts of zinc acetate, and 5-10 parts of ammonia water; S3: Preparation of short fiber composites: Take aramid nano short fibers and a dispersant, put them into a pulverizer and grind them for 20 to 30 minutes, take epoxy resin, and stir them at high speed for 20 to 30 minutes to obtain a short fiber composite; the ingredients are: 100 to 150 parts of aramid nano short fibers, 5 to 10 parts of dispersant, and 1 to 2 parts of epoxy resin in parts by weight; wherein the dispersant is polyethylene oxide, and the stirring speed is 1000 rad / min; S4: taking the prepared composite zinc oxide A, composite zinc oxide B, and short fiber composite, and blending them in a weight ratio of (1-1.5):(1-2):1 to obtain a highly dispersed nano zinc oxide for rubber; S5: Take styrene-butadiene rubber, high cis-1,4-butadiene rubber, accelerator, composite zinc oxide A, composite zinc oxide B, a blended product of a short fiber composite, microcrystalline wax, stearic acid, carbon black, and environmentally friendly oil, mix them to 150-160°C, then discharge the glue, stand for 4-5 hours, add sulfur and anti-scorch agent, and prepare highly dispersed nano zinc oxide rubber after the reaction is completed; the ingredients are: in parts by weight, 40-50 parts of styrene-butadiene rubber, 60-70 parts of high cis-1,4-butadiene rubber, 1-2 parts of accelerator, 1-2 parts of composite zinc oxide A, 1-2 parts of composite zinc oxide B, 1-2 parts of short fiber composite, 1-2 parts of microcrystalline wax, 0.5-1.5 parts of stearic acid, 55-60 parts of carbon black, 14-20 parts of environmentally friendly oil, 1-2 parts of sulfur, and 1-2 parts of anti-scorch agent; wherein the accelerator is NS and the anti-scorch agent is CTP.