A method for pre-sodiumization of sodium ion battery

By coating sodium tablets with glue in sodium ion batteries and pressurized at high temperature, the complexity of pre-sodiumization and large-scale production problems of existing sodium ion batteries are solved, and efficient sodium ion embedding and battery performance improvement are achieved.

CN117691205BActive Publication Date: 2024-11-05ANQING CHAOREN ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311758103.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-20
Publication Date
2024-11-05
Estimated Expiration
2043-12-20

AI Technical Summary

Technical Problem

The existing pre-sodiumization method of sodium ion batteries is complex and difficult to produce on a large scale. The first Coulomb efficiency is low, and a large amount of active sodium is consumed during the transformation stage, resulting in a decrease in the battery cell specific energy and an increase in cost.

Method used

Coat the sodium sheets with glue in a protective atmosphere. After forming glue, place them closely between the negative electrode sheet and the diaphragm. Pre-sodiumization is carried out through high-temperature pressure to ensure that the sodium sheet and the negative electrode sheet are in direct contact and avoid sodium oxidation. , suitable for large-scale production.

Benefits of technology

It significantly improves the first Coulomb efficiency and energy density of sodium ion batteries, simplifies operating steps, is suitable for large-scale production, and improves cycling performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the field of sodium ion batteries. In order to solve the problem that the pre-sodiumization operation of sodium ion batteries is complicated and difficult to mass produce under the prior art, a pre-sodiumization method of sodium ion batteries is provided, comprising the following steps: S1, under a protective atmosphere, using a glue solution to completely coat the surface of a sodium sheet, and drying to obtain a glue-coated sodium sheet; S2, when assembling a sodium ion battery, placing the glue-coated sodium sheet close to the negative electrode sheet between the negative electrode sheet and the diaphragm, and then winding to obtain a battery roll core; S3, baking the roll core after putting it into a shell, and performing high-temperature pressurization after liquid injection and aging of the seepage liquid to complete the pre-sodiumization. The method can significantly improve the first coulomb efficiency of a sodium ion battery and is suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of sodium ion batteries, and in particular to a method for pre-sodiumization of sodium ion batteries. Background Art

[0002] Sodium-ion batteries have developed rapidly in recent years due to their excellent performance and low cost, and their products have gradually been applied to electric two-wheeled vehicles, low-speed vehicles, energy storage and other fields. Although sodium and lithium have similar properties, graphite, which was previously used in the negative electrode of lithium-ion batteries, cannot be used in sodium-ion batteries. Currently, the negative electrode of sodium-ion batteries is generally based on amorphous carbon, that is, soft carbon and hard carbon. However, the main problem with amorphous carbon is that the initial coulomb efficiency is low, and a large amount of active sodium will be consumed in the formation stage, resulting in a decrease in the specific energy of the battery cell and an increase in cost.

[0003] At present, the main methods for improving amorphous carbon include: 1. Short-circuit pre-sodiumization, which is to squeeze the sodium sheet and the electrode to be treated, add a small amount of electrolyte, and migrate the sodium ions to the electrode surface through the potential difference between the two. The main disadvantage is that it is not easy to control the depth of pre-sodiumization, and the short-circuit process needs to prevent the sodium from being oxidized, which is not conducive to large-scale production; 2. Electrochemical pre-sodiumization is to assemble the sodium sheet and the electrode to be treated into a button battery, pre-sodiumize by controlling the charging current and voltage, and then disassemble the battery, take out the pre-sodiumized electrode and reuse it. The main disadvantage is that it can only be tried on small samples in the laboratory and cannot be mass-produced. 3. Chemical pre-sodiumization is a method of chemically supplementing sodium ion battery electrode materials with strongly reducing chemical reagents. The disadvantage is that there are reagent residues after pre-sodiumization, which affects the battery performance, and the chemical reagents cause a certain degree of pollution to the environment. For example, the invention patent with publication number CN115249795A soaks the negative electrode plate in a pre-sodiumization solution to obtain a pre-sodiumized negative electrode plate, and the pre-sodiumization solution contains aromatic hydrocarbon compounds including benzene, naphthalene, biphenyl, anthracene, kun, 2-methylbiphenyl, 4,4'-dimethylbiphenyl or 3,3',4,4'-tetramethylbiphenyl. 4. Positive electrode sodium supplementation additives are high-capacity irreversibly deintercalated sodium-rich compounds added to the positive electrode slurry. The disadvantage is that the compound requires a suitable decomposition potential, and some will produce flammable gases or introduce new impurities. Summary of the invention

[0004] In order to overcome the problem that the pre-sodiumization operation of sodium ion batteries is complicated and difficult to mass-produce under the prior art, the present invention provides a pre-sodiumization method for sodium ion batteries, which can significantly improve the first coulombic efficiency of sodium ion batteries and is suitable for mass production.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for pre-sodiumization of a sodium ion battery comprises the following steps:

[0007] S1. Under a protective atmosphere, the surface of the sodium sheet is completely coated with glue, and then dried to obtain a glue-coated sodium sheet;

[0008] S2. When assembling a sodium ion battery, the glue-coated sodium sheet is placed between the negative electrode sheet and the separator close to the negative electrode sheet, and then wound to obtain a battery roll core;

[0009] S3, baking the roll core after putting it into the shell, and then applying high temperature and pressure after liquid injection and aging to complete pre-sodiumization.

[0010] The present invention uses a sodium sheet to supplement sodium to the negative electrode of a sodium ion battery. First, a glue solution is used to coat the sodium sheet under a protective atmosphere, and then the organic solvent is dried to form a glue coating. After coating, the glue on the surface of the sodium sheet can isolate the sodium from contact with water or oxygen in the air to avoid sodium oxidation, so that subsequent production can be carried out in a conventional environment, and it is not necessary to operate in a protective atmosphere throughout the process, which is conducive to large-scale production. Then, the glue-coated sodium sheet is placed between the negative electrode sheet and the diaphragm to prepare a sodium ion battery, and the glue on the outside of the sodium sheet is melted by high temperature and pressure, so that the sodium sheet is in direct contact with the negative electrode sheet. Under the action of pressure and electrolyte, the sodium sheet at a high potential can be directly embedded in the negative electrode sheet in a low potential area to achieve the purpose of pre-sodiumization.

[0011] Preferably, the glue in S1 comprises a high molecular polymer and an organic solvent, and the mass of the high molecular polymer accounts for 1-3% of the mass of the glue.

[0012] Preferably, the high molecular polymer is one or more of polytetrafluoroethylene, polyethylene oxide, polyvinylidene fluoride and modified polyvinylidene fluoride.

[0013] Preferably, the modified polyvinylidene fluoride is polyethylene glycol blended polyvinylidene fluoride.

[0014] Preferably, the organic solvent is N-methylpyrrolidone.

[0015] Preferably, the thickness of the sodium sheet in S1 is 1-100 μm, and the thickness of the glue coating is 1-5 μm.

[0016] When the thickness of the glue coating is too small, the protection effect on the sodium sheet is poor, while when the thickness is too large, it will affect the melting effect under high temperature and pressure, and cause certain obstacles to the contact between the sodium sheet and the negative electrode.

[0017] Preferably, the high temperature pressurization in S3 is performed at a temperature of 65°C-90°C, a pressure of 0.4-1.0 MPa, and a time of 20-30 seconds.

[0018] Preferably, the S3 further comprises pre-forming charging after high temperature pressurization, wherein the pre-forming charging is a step charging of 0.05C-0.5C, the temperature during pre-forming is 35-55°C, and the pressure is 0.3-0.5MPa.

[0019] Preferably, the drying temperature in S1 is 90° C.-150° C., and the drying time is 120-300 seconds.

[0020] Preferably, the width of the sodium sheet in S1 is not greater than the width of the negative electrode coating area.

[0021] Preferably, the protective atmosphere in S1 is an inert atmosphere or a reducing atmosphere.

[0022] The inert atmosphere includes nitrogen and argon atmospheres, and the reducing atmosphere includes hydrogen atmosphere.

[0023] Therefore, the present invention has the following beneficial effects: (1) the pre-sodiumization effect is good, which can significantly improve the initial coulombic efficiency of the sodium ion battery; (2) the operation steps are simple, and it does not need to be carried out under a protective atmosphere throughout the process, and large-scale production is possible. DETAILED DESCRIPTION

[0024] The present invention is further described below in conjunction with specific implementation methods.

[0025] The sodium ion battery prepared in the following implementation method is a 10Ah aluminum-plastic film soft-package sodium ion battery, and the positive electrode roll is prepared by mixing sodium nickel iron manganese oxide, conductive carbon black and PVDF binder in a mass ratio of 94:3:3 in N-methylpyrrolidone, and after high-speed dispersion in a stirrer, it is evenly coated on an aluminum foil by a coater, and after drying in an oven, it is rolled and rolled up;

[0026] The negative electrode roll is made by mixing hard carbon, conductive carbon black and PVDF binder in N-methylpyrrolidone at a mass ratio of 94:3:3, dispersing them at high speed in a mixer, coating them evenly on aluminum foil by a coater, drying them in an oven, and rolling them up.

[0027] The diaphragm is PP;

[0028] The electrolyte was ethyl methyl carbonate containing 1 M NaPF6 and vinylene carbonate;

[0029] The specific method of 0.05C-0.5C step charging is: charge to 10% SOC at 0.05C constant voltage, then charge to 35% SOC at 0.1C constant voltage, and finally charge to 100% SOC at 0.5C.

[0030] Example 1

[0031] A method for pre-sodiumization of a sodium ion battery:

[0032] S1. Dissolve polytetrafluoroethylene in N-methylpyrrolidone at a mass fraction of 2 wt % to obtain a glue solution, and evenly apply the glue solution to each surface of a sodium sheet (thickness of 50 μm, width of 150 mm) under nitrogen atmosphere protection, with a coating thickness of 2 μm, dry at 90° C. for 120 s to completely cover the sodium sheet with the glue, and roll it up for standby use;

[0033] S2, winding the produced positive electrode roll, negative electrode roll, separator and the above-prepared glue-coated sodium sheet, wherein the negative electrode is closely attached to the coated sodium sheet;

[0034] S3, putting the wound core into a shell, baking, injecting liquid, and aging the liquid;

[0035] S4. Place the battery cell that has completed the infiltration into a high-temperature pressurized forming device, first perform high-temperature pressurization at a temperature of 65°C, a pressure of 1.0MPa, and a time of 20s; then perform pre-forming charging at a temperature of 35°C and a pressure of 0.3MPa, and use a step-by-step charging method of 0.05C-0.5C.

[0036] Example 2

[0037] A method for pre-sodiumization of a sodium ion battery:

[0038] S1. Dissolve polyvinylidene fluoride in N-methylpyrrolidone at a mass fraction of 2 wt % to obtain a glue solution, and evenly apply the glue solution to each surface of a sodium sheet (thickness of 50 μm, width of 150 mm) under nitrogen atmosphere protection, with a coating thickness of 1 μm, dry at 90° C. for 100 s to completely cover the sodium sheet with the glue, and roll it up for standby use;

[0039] S2, winding the produced positive electrode roll, negative electrode roll, separator and the above-prepared glue-coated sodium sheet, wherein the negative electrode is closely attached to the coated sodium sheet;

[0040] S3, putting the wound core into a shell, baking, injecting liquid, and aging the liquid;

[0041] S4. Place the battery cell that has completed the infiltration into a high-temperature pressurized forming device, first perform high-temperature pressurization at a temperature of 90°C, a pressure of 0.5MPa, and a time of 20s; then perform pre-forming charging at a temperature of 35°C and a pressure of 0.3MPa, and use a step-by-step charging method of 0.05C-0.5C.

[0042] Example 3

[0043] A method for pre-sodiumization of a sodium ion battery:

[0044] S1. Dissolve polyvinylidene fluoride in N-methylpyrrolidone at a mass fraction of 2 wt % to obtain a glue solution, and evenly apply the glue solution on each surface of a sodium sheet (thickness of 50 μm, width of 150 mm) under the protection of a nitrogen atmosphere, with a coating thickness of 5 μm, dry at 120° C. for 180 s to completely cover the sodium sheet with the glue, and roll it up for standby use;

[0045] S2, winding the produced positive electrode roll, negative electrode roll, separator and the above-prepared glue-coated sodium sheet, wherein the negative electrode is closely attached to the coated sodium sheet;

[0046] S3, putting the wound core into a shell, baking, injecting liquid, and aging the liquid;

[0047] S4. Place the battery cell that has completed the infiltration into a high-temperature pressurized forming device, first perform high-temperature pressurization at a temperature of 90°C, a pressure of 0.5MPa, and a time of 20s; then perform pre-forming charging at a temperature of 35°C and a pressure of 0.3MPa, and use a step-by-step charging method of 0.05C-0.5C.

[0048] Example 4

[0049] A method for pre-sodiumization of a sodium ion battery:

[0050] S1. Dissolve polyethylene glycol-blended polyvinylidene fluoride in N-methylpyrrolidone at a mass fraction of 3 wt % to obtain a glue solution, and evenly apply the glue solution on each surface of a sodium sheet (thickness of 50 μm, width of 150 mm) under nitrogen atmosphere protection, with a coating thickness of 3 μm, dry at 90° C. for 120 s to completely cover the sodium sheet with the glue, and roll it up for standby use;

[0051] S2, winding the produced positive electrode roll, negative electrode roll, separator and the above-prepared glue-coated sodium sheet, wherein the negative electrode is closely attached to the coated sodium sheet;

[0052] S3, putting the wound core into a shell, baking, injecting liquid, and aging the liquid;

[0053] S4. Place the battery cell that has completed the infiltration into a high-temperature pressurized forming device, first perform high-temperature pressurization at a temperature of 65°C, a pressure of 1.0MPa, and a time of 20s; then perform pre-forming charging at a temperature of 35°C and a pressure of 0.3MPa, and use a step-by-step charging method of 0.05C-0.5C.

[0054] Comparative Example 1

[0055] A method for pre-sodiumization of a sodium ion battery:

[0056] S1. Wind the produced positive electrode coil, negative electrode coil, separator and sodium sheet (thickness 50 μm, width 150 mm), wherein the negative electrode is close to the sodium sheet;

[0057] S2, putting the wound core into a shell, baking, injecting liquid, and aging the liquid;

[0058] S3. Place the battery cell that has completed the infiltration into a high-temperature pressurized forming device, first perform high-temperature pressurization at a temperature of 90°C, a pressure of 0.5MPa, and a time of 20s; then perform pre-forming charging at a temperature of 35°C and a pressure of 0.3MPa, and use a step-by-step charging method of 0.05C-0.5C.

[0059] Comparative Example 2

[0060] A method for pre-sodiumization of a sodium ion battery:

[0061] S1. Dissolve polyvinylidene fluoride in N-methylpyrrolidone at a mass fraction of 2 wt % to obtain a glue solution, and evenly apply the glue solution to each surface of a sodium sheet (thickness of 50 μm, width of 150 mm) under nitrogen atmosphere protection, with a coating thickness of 1 μm, dry at 90° C. for 100 s to completely cover the sodium sheet with the glue, and roll it up for standby use;

[0062] S2, winding the produced positive electrode roll, negative electrode roll, separator and the above-prepared glue-coated sodium sheet, wherein the negative electrode is closely attached to the coated sodium sheet;

[0063] S3, putting the wound core into a shell, baking, injecting liquid, and aging the liquid;

[0064] S4. The battery cell that has been infiltrated is pre-charged. The temperature during pre-charging is 35°C and the pressure is 0.3MPa. The charging adopts 0.05C-0.5C step charging.

[0065] Comparative Example 3

[0066] A method for pre-sodiumization of a sodium ion battery:

[0067] S1. Dissolve polyvinylidene fluoride in N-methylpyrrolidone at a mass fraction of 2 wt % to obtain a glue solution, and evenly apply the glue solution to each surface of a sodium sheet (thickness of 50 μm, width of 150 mm) under nitrogen atmosphere protection, with a coating thickness of 10 μm, dry at 130° C. for 300 s to completely cover the sodium sheet with the glue, and roll it up for standby use;

[0068] S2, winding the produced positive electrode roll, negative electrode roll, separator and the above-prepared glue-coated sodium sheet, wherein the negative electrode is closely attached to the coated sodium sheet;

[0069] S3, putting the wound core into a shell, baking, injecting liquid, and aging the liquid;

[0070] S4. Place the battery cell that has completed the infiltration into a high-temperature pressurized forming device, first perform high-temperature pressurization at a temperature of 90°C, a pressure of 0.5MPa, and a time of 20s; then perform pre-forming charging at a temperature of 35°C and a pressure of 0.3MPa, and use a step-by-step charging method of 0.05C-0.5C.

[0071] Comparative Example 4

[0072] A method for pre-sodiumization of a sodium ion battery:

[0073] S1. Dissolve polyvinylidene fluoride in N-methylpyrrolidone at a mass fraction of 2 wt % to obtain a glue solution, and evenly apply the glue solution to each surface of a sodium sheet (thickness of 50 μm, width of 150 mm) under nitrogen atmosphere protection, with a coating thickness of 5 μm, dry at 120° C. for 280 s to completely cover the sodium sheet with the glue, and roll it up for standby use;

[0074] S2, winding the produced positive electrode roll, negative electrode roll, separator and the above-prepared glue-coated sodium sheet, wherein the negative electrode is closely attached to the coated sodium sheet;

[0075] S3, putting the wound core into a shell, baking, injecting liquid, and aging the liquid;

[0076] S4. Place the battery cell that has completed the infiltration into a high-temperature pressurized forming device, first perform high-temperature pressurization at a temperature of 130°C, a pressure of 0.5MPa, and a time of 60s; then perform pre-forming charging at a temperature of 35°C and a pressure of 0.3MPa, and use a step-by-step charging method of 0.05C-0.5C.

[0077] The first-week coulombic efficiency, energy density and cycle performance of the pre-sodiumized sodium ion batteries obtained in the above embodiments and comparative examples were tested, wherein the cycle performance was characterized by the capacity retention rate after 200 cycles at a 1C rate. The test results are shown in the following table.

[0078] project First week coulomb efficiency % Energy densityWh / kg Capacity retention rate after 200 weeks % Example 1 96.7 142 98.8 Example 2 96.6 144 98.2 Example 3 97.1 140 99.1 Example 4 97.5 142 98.4 Comparative Example 1 74.9 108 84.6 Comparative Example 2 81.5 117 85.9 Comparative Example 3 80.4 115 85.3 Comparative Example 4 74.3 106 80.9

[0079] It can be seen from the above table that the pre-sodiumization effect of the present invention is good, and the first coulombic efficiency, energy density and cycle performance of the sodium ion battery can be significantly improved.

[0080] In Comparative Example 1, no glue-coated sodium sheet was used, resulting in oxidation of the sodium sheet in the subsequent production process, and sodium oxide could not participate in pre-sodiumization, and even formed a sodium oxide layer on the surface of the negative electrode to hinder the embedding and removal of sodium ions. In Comparative Example 2, the glue-coated sodium sheet was only pre-formed after being attached to the negative electrode without high-temperature pressurization. The glue layer hindered the embedding of the sodium sheet into the negative electrode, resulting in poor pre-sodiumization effect. The glue coating layer of Comparative Example 3 was too thick, and the glue layer was not completely removed during the high-temperature pressurization process, resulting in poor pre-sodiumization effect. In Comparative Example 4, a higher temperature was used in the high-temperature pressurization. Although the removal effect of the glue was good, the excessively high temperature had a greater negative impact on the electrolyte, resulting in a decrease in performance after pre-sodiumization.

Claims

1. A method for pre-sodiumization of a sodium ion battery, characterized in that it comprises the steps of: S1. Under a protective atmosphere, the surface of the sodium sheet is completely coated with glue, and then dried to obtain a glue-coated sodium sheet; S2. When assembling a sodium ion battery, the glue-coated sodium sheet is placed between the negative electrode sheet and the separator close to the negative electrode sheet, and then wound to obtain a battery roll core; S3. After the roll core is put into the shell, it is baked. After the liquid is injected and aged, it is pressurized at high temperature to melt the glue to complete the pre-sodiumization.

2. A method for pre-sodiumization of a sodium ion battery according to claim 1, Its characteristics are: The glue solution in S1 includes a high molecular polymer and an organic solvent, and the mass of the high molecular polymer accounts for 1-3% of the mass of the glue solution.

3. A method for pre-sodiumization of a sodium ion battery according to claim 2, Its characteristics are: The high molecular polymer is one or more of polytetrafluoroethylene, polyethylene oxide, polyvinylidene fluoride and modified polyvinylidene fluoride.

4. A method for pre-sodiumization of a sodium ion battery according to claim 2, Its characteristics are: The organic solvent is N-methylpyrrolidone.

5. A method for pre-sodiumization of a sodium ion battery according to claim 1, 2 or 4, Its characteristics are: The thickness of the sodium sheet in S1 is 1-100 μm, and the thickness of the glue coating is 1-5 μm.

6. A method for pre-sodiumization of a sodium ion battery according to claim 5, Its characteristics are: The temperature of the high temperature pressurization in S3 is 65° C.-90° C., the pressure is 0.4-1.0 MPa, and the time is 20-30 seconds.

7. A method for pre-sodiumization of a sodium ion battery according to claim 1, Its characteristics are: The S3 also includes pre-charging after high temperature pressurization, the pre-charging is a step charging of 0.05C-0.5C, the temperature during pre-charging is 35-55°C, and the pressure is 0.3-0.5MPa.

8. A method for pre-sodiumization of a sodium ion battery according to claim 1, Its characteristics are: The drying temperature in S1 is 90° C.-150° C. and the drying time is 120-300 seconds.

9. A method for pre-sodiumization of a sodium ion battery according to claim 1, Its characteristics are: The width of the sodium sheet in S1 is not greater than the width of the negative electrode coating area.

10. A method for pre-sodiumization of a sodium ion battery according to claim 1, Its characteristics are: The protective atmosphere in S1 is an inert atmosphere or a reducing atmosphere.