A kind of unburned brick of full solid waste system based on waste mud and preparation method thereof
By mixing waste mud, desulfurization gypsum, alkali activator and slag in a specific proportion to prepare burn-free bricks, the problem of increased workload and low dosage of dehydration treatment in the existing technology is solved, achieving efficient use of waste materials and reducing energy consumption. and environmental pollution, producing high-strength, durable, no-fire bricks, in line with the concept of low-carbon environmental protection.
Patent Information
- Application Number
- CN202311718906.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-13
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-12-13
AI Technical Summary
The existing technology requires dehydration treatment when using waste slurry to prepare burn-free bricks, which increases the workload and energy consumption. The amount of waste materials is low, which is not conducive to the comprehensive utilization of bulk solid waste, and the process is complex and requires pressing and sintering.
The unfired bricks are prepared by using the ratio of 70 to 80% waste mud, 5 to 10% desulfurized gypsum, 5 to 8% alkali activator, and 10 to 20% slag. After mixing, they are aged and solidified, and combined with high moisture content waste mud. Characteristics: avoid firing and mechanical pressing, and adopt low-temperature and low-humidity maintenance conditions.
It achieves efficient utilization of waste slurry and industrial solid waste, reduces energy consumption and environmental pollution, and produces burn-free bricks with high strength and durability, which meets the requirements of low-carbon green and environmentally friendly development, and has a simple process and low cost.
Smart Images

Figure CN117700191B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of waste treatment and resource recycling, and in particular to an unburned brick of a full solid waste system based on waste mud and a preparation method thereof. Background Art
[0002] The development of urban underground space construction, dredging projects, island and reef projects, etc. will generate a large amount of waste mud. The current method of large-scale treatment of waste mud is to collect soil to build a dump for temporary or permanent storage. Due to the poor engineering properties of waste mud, waste mud dumps require long-term and large-scale land use, which will also cause environmental pollution. In the current situation of limited land space resources and increasingly harsh ecological environment, how to safely handle and reasonably utilize the growing amount of waste mud and turn it into treasure is directly related to the quality of human living environment and the sustainable development of society and economy.
[0003] At the same time, industrial activities will generate a large amount of solid waste such as blast furnace slag, industrial by-product desulfurization gypsum, etc. The current comprehensive utilization rate of these materials is not high, and they have not been effectively utilized. Large-scale accumulation will cause environmental pollution and waste of resources. In addition, in the existing process of preparing unburned bricks using waste mud, the waste mud needs to be dehydrated, which greatly increases the workload. At the same time, in the existing process of preparing unburned bricks using waste materials, the amount of waste materials added is small, which is not conducive to the comprehensive utilization of waste materials. Therefore, this field urgently needs to develop a method for preparing unburned bricks using waste materials with a high amount of waste materials and without the need for pre-treatment of the waste mud. Summary of the invention
[0004] The purpose of the present invention is to provide a fired-free brick based on a full solid waste system of waste mud and a preparation method thereof, so as to solve the problems that in the existing process of preparing fired-free bricks using waste materials, the waste mud needs to be dehydrated, which increases the workload and energy consumption, the low content of waste materials is not conducive to the comprehensive utilization of "bulk solid waste", and the preparation process is complicated and requires pressing and sintering.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] The present invention provides an unburned brick of a full solid waste system based on waste mud, which is prepared from raw materials containing the following parts by weight: 70-80 parts of waste mud, 5-10 parts of desulfurized gypsum, 5-8 parts of alkali activator, and 10-20 parts of slag.
[0007] Preferably, the water content of the waste sludge is 100-120%.
[0008] Preferably, the particle size of the desulfurized gypsum is ≤0.08 mm.
[0009] Preferably, the alkaline activator is magnesium oxide, and the particle size of the alkaline activator is ≤0.08 mm.
[0010] Preferably, the slag is S95 grade slag powder, and the particle size of the slag is 46-100 μm.
[0011] The present invention also provides a method for preparing the unburned bricks of the full solid waste system based on waste mud, comprising the following steps:
[0012] The waste mud, desulfurized gypsum, alkali activator and slag are mixed and aged to obtain a mixture; the mixture is solidified and formed and then cured to obtain unburned bricks.
[0013] Preferably, the waste mud is sieved before mixing, and the aperture of the sieve used for sieving is 8 to 12 meshes.
[0014] Preferably, the desulfurized gypsum, alkali activator and slag are sieved separately before mixing, and the aperture of the sieve used for sieving is independently 200-270 meshes.
[0015] Preferably, the aging time is 6 to 10 hours; the curing molding is carried out in a mold, the curing molding temperature is 18 to 22° C., and the curing molding time is 24 to 48 hours.
[0016] Preferably, the curing temperature is 18-22° C., the curing humidity is ≥90%, and the curing time is 26-30 days.
[0017] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0018] (1) The present invention can digest waste mud to a great extent, solve the problem of waste of resources and environmental pollution caused by long-term and large-scale use of land in waste mud yards, high cost, large carbon emissions and environmental pollution in large-scale resource treatment of waste mud, and at the same time use the full solid waste solidification system to treat waste mud, achieve the comprehensive utilization goal of "waste treatment", and meet the economic concept of low-carbon green environmental protection development; the present invention adopts high-water content waste mud and non-burning process, fully utilizes the high water content and excellent fluidity of waste mud itself, does not need to be burned and mechanically pressed, is conducive to reducing energy consumption, and reduces environmental problems caused by the burning process, meeting the requirements of energy conservation and emission reduction;
[0019] (2) The present invention uses bulk solid waste slag and desulfurized gypsum generated in industrial activities, and uses these materials to treat waste mud to prepare unburned bricks, which can promote the comprehensive utilization of "bulk solid waste" and achieve green, efficient, high-quality, high-value, and large-scale utilization. At the same time, the present invention does not use cement-based high-carbon emission materials to treat waste mud, and does not require firing and mechanical pressing, which is in line with the concept of environmental protection and responds to the call of the national dual-carbon strategy;
[0020] (3) The present invention uses high-water content waste mud, desulfurized gypsum, alkali activator and slag as main raw materials. The unburned bricks produced have high strength, good durability, good water stability, simple process and low cost. After curing, the compressive strength is above 15MPa and can reach MU15 grade. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0022] Figure 1 This is a process flow chart of the preparation of the unfired bricks of the present invention;
[0023] Figure 2 This is a schematic diagram of the preparation process of the unfired brick described in Example 1;
[0024] Figure 3 These are the three views of the brick mold used, where a is the three views of the brick mold body, b is the three views of the brick mold bottom cover, and c is the three views of the brick mold top cover. DETAILED DESCRIPTION
[0025] The present invention provides an unburned brick of a full solid waste system based on waste mud, which is prepared from raw materials containing the following parts by weight: 70-80 parts of waste mud, 5-10 parts of desulfurized gypsum, 5-8 parts of alkali activator, and 10-20 parts of slag.
[0026] In the present invention, the amount of the waste mud is preferably 72 to 78 parts, more preferably 73 to 76 parts, and more preferably 74 to 75 parts; the amount of the desulfurized gypsum is preferably 6 to 9 parts, more preferably 6.5 to 8.5 parts, and more preferably 7 to 8 parts; the amount of the alkali activator is preferably 5.5 to 7.5 parts, more preferably 6 to 7 parts, and more preferably 6.5 parts; the amount of the slag is preferably 12 to 18 parts, more preferably 13 to 17 parts, and more preferably 15 to 16 parts.
[0027] In the present invention, the waste mud is selected from waste mud from urban underground space construction, dredging projects, island and reef projects, shield excavation projects and other projects; the water content of the waste mud is preferably 100-120%, more preferably 105-115%, and more preferably 110-112%.
[0028] In the present invention, the particle size of the desulfurized gypsum is preferably ≤0.08 mm, more preferably ≤0.07 mm, and more preferably ≤0.05 mm.
[0029] In the present invention, the alkaline activator is preferably magnesium oxide, and the particle size of the alkaline activator is preferably ≤0.08 mm, more preferably ≤0.06 mm, and more preferably ≤0.05 mm.
[0030] In the present invention, the slag is preferably S95 grade slag powder, and the particle size of the slag is preferably 46 to 100 μm, more preferably 50 to 95 μm, and more preferably 80 to 90 μm.
[0031] The present invention also provides a method for preparing the unburned bricks of the full solid waste system based on waste mud, comprising the following steps:
[0032] The waste mud, desulfurized gypsum, alkali activator and slag are mixed and aged to obtain a mixture; the mixture is solidified and formed and then cured to obtain unburned bricks.
[0033] In the present invention, the waste mud is sieved before mixing, and the aperture of the sieve used for sieving is preferably 8-12 meshes, and more preferably 10 meshes; after sieving, the sieve underfill is taken.
[0034] In the present invention, the desulfurized gypsum, alkali activator and slag are sieved separately before mixing, and the aperture of the sieve used for sieving is preferably 200-270 mesh, and more preferably 230 mesh; after sieving, the sieve underfill is taken.
[0035] In the present invention, the desulfurized gypsum, alkali activator and slag are dried and ground separately before screening; the drying temperature is independently preferably 20-26°C, more preferably 22-25°C, and more preferably 23-24°C; the drying time is independently preferably 3-6h, more preferably 4-5h, and more preferably 4.5h.
[0036] In the present invention, the stirring speed of the mixing is preferably 800-1200 r / min, more preferably 900-1100 r / min, more preferably 1000 r / min; the mixing time is preferably 20-40 min, more preferably 25-35 min, more preferably 30 min.
[0037] In the present invention, the aging time is preferably 6 to 10 hours, more preferably 7 to 9 hours, and more preferably 8 hours; the aged material is turned over during the aging period; the number of turnings is preferably 3 to 5 times, and more preferably 4 times.
[0038] In the present invention, the curing molding is carried out in a mold; the mold is a brick mold; the brick mold includes a brick mold body, a brick mold bottom cover and a brick mold top cover; the curing molding temperature is preferably 18-22°C, further preferably 19-21°C, and more preferably 20°C; the curing molding time is preferably 24-48h, further preferably 30-42h, and more preferably 36-40h.
[0039] In the present invention, the curing temperature is preferably 18-22°C, more preferably 19-21°C, and more preferably 20°C; the curing humidity is preferably ≥90%, more preferably ≥92%, and more preferably ≥95%; the curing time is preferably 26-30d, more preferably 27-29d, and more preferably 28d.
[0040] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0041] The parts described in the following examples are all parts by mass.
[0042] Example 1
[0043] The raw materials used in this embodiment and their amounts are as follows: 75 parts of waste mud with a moisture content of 105% produced by dredging projects, 5 parts of desulfurized gypsum with a particle size of ≤0.08 mm, 5 parts of magnesium oxide with a particle size of ≤0.08 mm, and 15 parts of S95 grade slag powder with a particle size of 95 μm.
[0044] The preparation process is as follows:
[0045] The waste mud with a moisture content of 105% is sieved, and the aperture of the sieve used is 10 meshes to remove weeds, small stones and other debris in the waste mud; the desulfurized gypsum with a particle size of ≤0.08mm, the magnesium oxide with a particle size of ≤0.08mm and the S95 grade slag powder with a particle size of 95μm are dried at 22°C for 6h, and then ground separately, and finally sieved separately, and the aperture of the sieve used is 200 meshes, and mixed after sieving to obtain a mixed powder; the mixed powder and the sieved waste mud are placed in a mixer, and Mix for 40 minutes at a rotation speed of 1200r / min, then place in a dry and ventilated place for aging for 6 hours, turning over 4 times during the aging period; pour the aged material into a brick mold (the brick mold is a 95 standard brick mold with dimensions (length × width × height) of 240 × 115 × 53mm and a tolerance of ±2mm), and cure at 20°C for 40 hours; take out the cured brick along the direction of the brick mold groove, and cure at a temperature of 20°C and a humidity of 92% for 28 days to obtain unfired bricks.
[0046] The properties of the unfired brick obtained in this example were tested. According to the test, the compressive strength of the unfired brick was 17 MPa, the water absorption rate was 15%, and the softening coefficient was 0.8.
[0047] Example 2
[0048] The raw materials used in this embodiment and their amounts are as follows: 70 parts of waste mud with a moisture content of 105% generated by shield excavation engineering, 10 parts of desulfurized gypsum with a particle size of ≤0.08 mm, 5 parts of magnesium oxide with a particle size of ≤0.08 mm, and 15 parts of S95 grade slag powder with a particle size of 95 μm.
[0049] The preparation process is as follows:
[0050] The waste mud with a moisture content of 105% is sieved, and the aperture of the sieve used is 10 meshes to remove weeds, small stones and other debris in the waste mud; the desulfurized gypsum with a particle size of ≤0.08mm, the magnesium oxide with a particle size of ≤0.08mm and the S95 grade slag powder with a particle size of 95μm are dried at 20°C for 5h, and then ground separately, and finally sieved separately, and the aperture of the sieve used is 200 meshes, and mixed after sieving to obtain a mixed powder; the mixed powder and the sieved waste mud are placed in a mixer, and Mix for 40 minutes at a rotation speed of 1200r / min, then place in a dry and ventilated place for aging for 7 hours, turning over 5 times during the aging period; pour the aged material into a brick mold (the brick mold is a 95 standard brick mold with dimensions (length × width × height) of 240 × 115 × 53mm and a tolerance of ±2mm), and cure at 20°C for 36 hours; take out the cured brick along the direction of the brick mold groove, and cure at a temperature of 22°C and a humidity of 95% for 28 days to obtain unfired bricks.
[0051] The properties of the unfired brick obtained in this example were tested. According to the test, the compressive strength of the unfired brick was 16 MPa, the water absorption rate was 17%, and the softening coefficient was 0.8.
[0052] Example 3
[0053] The raw materials used in this embodiment and their amounts are as follows: 75 parts of waste mud with a moisture content of 115% produced by dredging projects, 5 parts of desulfurized gypsum with a particle size of ≤0.08 mm, 5 parts of magnesium oxide with a particle size of ≤0.08 mm, and 15 parts of S95 grade slag powder with a particle size of 95 μm.
[0054] The preparation process is as follows:
[0055] The waste mud with a moisture content of 115% is sieved, and the aperture of the sieve used is 10 meshes to remove weeds, small stones and other debris in the waste mud; the desulfurized gypsum with a particle size of ≤0.08mm, the magnesium oxide with a particle size of ≤0.08mm and the S95 grade slag powder with a particle size of 95μm are dried at 20°C for 5h, and then ground separately, and finally sieved separately, and the aperture of the sieve used is 200 meshes, and mixed after sieving to obtain a mixed powder; the mixed powder and the sieved waste mud are placed in a mixer, and Mix for 40 minutes at a speed of 800r / min, then place in a dry and ventilated place for aging for 10 hours, turning over 3 times during the aging period; pour the aged material into a brick mold (the brick mold is a 95 standard brick mold with dimensions (length × width × height) of 240 × 115 × 53mm and a tolerance of ±2mm), and cure at 20°C for 24 hours; take out the cured brick along the direction of the brick mold groove, and cure at a temperature of 18°C and a humidity of 90% for 28 days to obtain unfired bricks.
[0056] The properties of the unfired brick obtained in this example were tested. According to the test, the compressive strength of the unfired brick was 15 MPa, the water absorption rate was 19%, and the softening coefficient was 0.8.
[0057] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A kind of unburned brick based on waste mud and full solid waste system, It is characterized in that The method is prepared from the following raw materials in parts by weight: 70-80 parts of waste mud, 5-10 parts of desulfurized gypsum, 5-8 parts of alkali activator, and 10-20 parts of slag; The water content of the waste mud is 100-120%; The alkaline activator is magnesium oxide.
2. The unburned brick of the full solid waste system based on waste mud according to claim 1, It is characterized in that The particle size of the desulfurized gypsum is ≤0.08 mm.
3. The unburned brick of the full solid waste system based on waste mud according to claim 1 or 2, It is characterized in that The alkaline activator is magnesium oxide, and the particle size of the alkaline activator is ≤0.08 mm.
4. The unburned brick of the full solid waste system based on waste mud according to claim 3, It is characterized in that The slag is S95 grade slag powder, and the particle size of the slag is 46-100 μm.
5. The method for preparing unburned bricks of the full solid waste system based on waste mud according to any one of claims 1 to 4, It is characterized in that The steps include: The waste mud, desulfurized gypsum, alkali activator and slag are mixed and aged to obtain a mixture; the mixture is solidified and formed and then cured to obtain unburned bricks.
6. The method for preparing unburned bricks of the full solid waste system based on waste mud according to claim 5, It is characterized in that The waste mud is sieved before mixing, and the aperture of the sieve used for sieving is 8 to 12 meshes.
7. The method for preparing unburned bricks of the full solid waste system based on waste mud according to claim 6, It is characterized in that The desulfurized gypsum, alkali activator and slag are sieved separately before mixing, and the aperture of the sieve used for sieving is independently 200-270 meshes.
8. The method for preparing unburned bricks of the full solid waste system based on waste mud according to claim 6 or 7, It is characterized in that The aging time is 6 to 10 hours; the curing molding is carried out in a mold, the curing molding temperature is 18 to 22° C., and the curing molding time is 24 to 48 hours.
9. The method for preparing unburned bricks of the full solid waste system based on waste mud according to claim 8, It is characterized in that The curing temperature is 18-22° C., the curing humidity is ≥90%, and the curing time is 26-30 days.
Citation Information
Patent Citations
Autoclaved / steam cured brick prepared from industrial waste and preparation process thereof
CN102408208A
Method for preparing baking-free slag brick
CN103193443A
Building baking-free bricks and production method thereof
CN103449775A
Green environment-friendly baking-free brick and preparation method thereof
CN106278088A
Baking-free brick prepared from waste slurry and preparation method thereof
CN107840623A