Compositions for preparing high-temperature resistant silica gel, high-temperature resistant silica gel and its preparation method, power module and its preparation method.
By using a composition of phenyl boron-containing vinyl silicone oil, phenyl-side hydrogen-containing silicone oil, platinum catalyst and inhibitor, a silicone gel with phenyl and boron-oxygen bonds is formed, which solves the problem of insufficient high-temperature resistance of existing silicone gels and realizes the packaging requirements of SiC-based electronic components at high temperatures.
Patent Information
- Application Number
- CN202211083972.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-06
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-09-06
AI Technical Summary
Existing silicone gels cannot meet the requirements of SiC-based electronic components for long-term use at high temperatures, thus limiting their application in power modules.
A composition of phenyl boron-containing vinyl silicone oil, phenyl-side hydrogen-containing silicone oil, platinum catalyst and inhibitor is used. By adjusting the proportion of each component, a silicone gel with phenyl and boron-oxygen bonds is formed during the heating and curing process, thereby improving its high temperature resistance.
The prepared silica gel has excellent high-temperature resistance and is suitable for the packaging of SiC-based electronic components, meeting the requirements of high-power modules to operate for extended periods at high temperatures.
Smart Images

Figure CN117701003B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of silica gel technology, and more specifically, to a composition for preparing high-temperature resistant silica gel, a high-temperature resistant silica gel and a method for preparing the same, and a power module and a method for preparing the same. Background Technology
[0002] A power module is a module formed by combining power electronic components according to certain functions and then encapsulating them; the encapsulation material is generally silicone gel.
[0003] With the continuous development of the electronic components industry, silicon carbide (SiC)-based semiconductor devices are increasingly favored by the industry due to their excellent properties such as high temperature resistance, high voltage resistance, and high frequency operation. SiC-based electronic devices have high power, which leads to more heat generation during operation (i.e., higher ambient temperature during operation).
[0004] However, the high-temperature resistance of existing silicone gels cannot meet the heat generation requirements of SiC-based electronic components during operation, which is not conducive to the long-term use of power modules at high temperatures and greatly limits the application of SiC-based electronic components in power modules. Summary of the Invention
[0005] The purpose of this application is to provide a composition for preparing high-temperature resistant silicone gel, a high-temperature resistant silicone gel and a method for preparing the same, and a power module and a method for preparing the same, which aims to improve the technical problem of poor high-temperature resistance of existing silicone gels.
[0006] In a first aspect, this application provides a composition for preparing high-temperature resistant silicone gel, comprising: phenyl boron-containing vinyl silicone oil, phenyl-side hydrogen-containing silicone oil, platinum catalyst, and inhibitor.
[0007] The mass ratio of phenyl boron-containing vinyl silicone oil, phenyl-side hydrogen-containing silicone oil, platinum catalyst and inhibitor is (10-20):(0.05-0.75):(0.06-0.4):(0.02-0.06).
[0008] The structural formula of phenyl boron-containing vinyl silicone oil is as follows:
[0009]
[0010] Where m and n are each an independent natural number greater than or equal to 1.
[0011] The structural formula of the phenyl-side hydrogen-containing silicone oil is as follows:
[0012]
[0013] In this context, x and y are each independent natural numbers greater than or equal to 1.
[0014] This application uses phenyl boron-containing vinyl silicone oil, phenyl-side hydrogen-containing silicone oil, platinum catalyst, and inhibitor, and adjusts the ratio of each component as a composition for preparing high-temperature resistant silicone gel. During the subsequent heating and curing process to prepare silicone gel, the inhibitor volatilizes and overflows from the system. Then, under the action of the platinum catalyst, the silicon-hydrogen bonds (-SiH) of the phenyl-side hydrogen-containing silicone oil break and undergo an addition curing reaction with the phenyl boron-containing vinyl silicone oil. This results in the silicone gel having both heat-resistant phenyl groups and high-bond-energy boron-oxygen bonds (BO) on the main chain, which is beneficial to improving the high-temperature resistance of the silicone gel.
[0015] In some embodiments of the first aspect of this application, the molar ratio of silane-hydrogen groups to silane-vinyl groups in the composition is (1-1.5):1.
[0016] The above ratio is beneficial to further improve the high temperature resistance and flexibility of the subsequently prepared silicone gel. If the content of silyl vinyl group (-SiCH=CH2) in the composition is too high, the silicone gel formed after addition curing will contain a large amount of unreacted silyl vinyl group. Since silyl vinyl group has poor stability at high temperature, it will undergo thermo-oxidative degradation, which will make the silicone gel harden. If the content of silane group (-SiH) in the composition is too high, the reaction between the components will not be sufficient, which is also not conducive to further improving the high temperature resistance of the prepared silicone gel.
[0017] Optionally, the vinyl content in the phenyl boron-containing vinyl silicone oil is 0.28-0.32 mmol / g; the phenyl content in the phenyl boron-containing vinyl silicone oil is 8-30 mol%.
[0018] Optionally, the hydrogen content in the phenyl-side hydrogen-containing silicone oil is 1-8.5 mmol / g; the phenyl content in the phenyl-side hydrogen-containing silicone oil is 30-50 mol%.
[0019] Optionally, the viscosity of the phenyl boron-containing vinyl silicone oil is 800-2500 mPa·s.
[0020] Optionally, the viscosity of the phenyl-side hydrogen-containing silicone oil is 2.5-400 mPa·s.
[0021] In some embodiments of the first aspect of this application, the composition further includes phenyl vinyl silicone oil; the mass ratio of phenyl vinyl silicone oil to phenyl boron-containing vinyl silicone oil is (32.5-60):(10-20).
[0022] Under the above circumstances, it is beneficial to further improve the high-temperature resistance of the subsequently prepared silicone gel by increasing the content of phenyl groups.
[0023] Optionally, the vinyl content in the phenyl vinyl silicone oil is 0.13-0.7 mmol / g; the phenyl content in the phenyl vinyl silicone oil is ≥35 mol%.
[0024] Optionally, the viscosity of the phenyl vinyl silicone oil is 600-3000 mPa·s.
[0025] In some embodiments of the first aspect of this application, the composition further includes a phenyl-terminated hydrogen-containing silicone oil; the mass ratio of the phenyl-terminated hydrogen-containing silicone oil to the phenyl-terminated hydrogen-containing silicone oil is (0.5-5):(0.05-0.75).
[0026] The structural formula of phenyl-terminated hydrogen-containing silicone oil is as follows:
[0027]
[0028] Where v and w are each an independent natural number greater than or equal to 1.
[0029] The addition of phenyl-terminated hydrogen-containing silicone oil is beneficial to improving the toughness of the subsequently prepared silicone gel; it is also beneficial to improve the adhesion performance of the subsequently prepared silicone gel. When silicone gel is used to encapsulate power electronic components, it can improve the adhesion between the silicone gel and the power module shell and the components, thereby improving the structural stability of the power module.
[0030] Optionally, the hydrogen content in the phenyl-terminated hydrogen-containing silicone oil is 3-6 mmol / g; the phenyl content in the phenyl-terminated hydrogen-containing silicone oil is 40-60 mol%.
[0031] Optionally, the viscosity of the phenyl-terminated hydrogen-containing silicone oil is 5-200 mPa·s.
[0032] In some embodiments of the first aspect of this application, the composition further includes cage-type polysilsesquioxane; the mass ratio of cage-type polysilsesquioxane to phenyl boron-containing vinyl silicone oil is (20-40):(10-20).
[0033] Cage-type polysilsesquioxane has a three-dimensional structure formed by a large number of Si-O-Si bonds. The addition of cage-type polysilsesquioxane is beneficial to further improve the high temperature resistance of silica gel through a large number of inorganic Si-O bonds.
[0034] Optionally, the cage-type polysilsesquioxane is selected from glycidyl-cage-type polysilsesquioxane.
[0035] Optionally, the viscosity of the cage-type polysilsesquioxane is 3500-4800 mPa·s.
[0036] In some embodiments of the first aspect of this application, the composition further includes a heat resistant agent; the heat resistant agent includes rare earth metal complexes; the mass ratio of the heat resistant agent to phenyl boron-containing vinyl silicone oil is (1-5):(10-20).
[0037] Rare earth metal complexes are selected as heat-resistant agents. The introduction of rare earth metal complexes will not affect the transparency of the silicone gel. At the same time, rare earth metal complexes can prevent free radical reactions caused by oxidation in the silicone gel at high temperatures. They can be regenerated in the presence of oxygen in the air. Moreover, they can absorb some acidic or alkaline substances in the silicone gel that can catalyze degradation reactions, thereby playing a role in thermal stability of the silicone gel. This achieves the purpose of preventing the oxidative crosslinking of polysiloxane side chains and the cyclization degradation of the main chain, which is beneficial to extending the service life of the silicone gel at high temperatures.
[0038] Optionally, the heat-resistant agent is a cerium oxide rare earth complex.
[0039] Optionally, the inhibitor is selected from alkynyl alcohol inhibitors, including at least one of 1-ethynyl-1-cyclohexanol, 3,7,11-trimethyldodecyn-3-ol, 3,5-dimethyl-1-hexyn-3-ol, and 2-methyl-3-butyn-3-ol.
[0040] In a second aspect, this application provides a method for preparing a high-temperature resistant silicone gel, comprising: curing the composition for preparing a high-temperature resistant silicone gel provided in the first aspect above at 110-130°C.
[0041] The composition for preparing high-temperature resistant silicone gel provided in the first aspect is cured at 110-130°C. The resulting silicone gel has excellent high-temperature resistance and can be used as a silicone gel for packaging high-power electronic components such as SiC-based components to meet the needs of high-power modules that generate a lot of heat and need to work at high temperatures for a long time.
[0042] Optionally, the method for preparing the composition includes: mixing a first raw material and a second raw material under vacuum conditions; wherein the first raw material comprises, by weight, 20-40 parts of phenyl boron-containing vinyl silicone oil and 0.12-0.8 parts of platinum catalyst; and the second raw material comprises, by weight, 0.1-1.5 parts of phenyl-side hydrogen-containing silicone oil and 0.04-0.12 parts of inhibitor.
[0043] Optionally, the first raw material may also include 60-80 parts by weight of phenyl vinyl silicone oil.
[0044] Optionally, the second ingredient may also include 5-40 parts by weight of phenyl vinyl silicone oil.
[0045] Optionally, the second raw material further includes 1-10 parts by weight of phenyl-terminated hydrogen-containing silicone oil; the structural formula of the phenyl-terminated hydrogen-containing silicone oil is as follows:
[0046]
[0047] Where v and w are each an independent natural number greater than or equal to 1.
[0048] Optionally, the second raw material may also include 40-80 parts by weight of cage-type polysilsesquioxane.
[0049] Optionally, the second raw material may also include 2-10 parts by weight of a heat-resistant agent; the heat-resistant agent may include rare earth metal complexes.
[0050] Thirdly, this application provides a high-temperature resistant silicone gel, which is prepared by the method for preparing high-temperature resistant silicone gel as described in the second aspect above.
[0051] The high-temperature resistant silicone gel provided in this application has excellent high-temperature resistance and can be used as a silicone gel for encapsulating high-power electronic components such as SiC-based devices to meet the needs of high-power modules that generate a lot of heat and need to operate at high temperatures for a long time.
[0052] Fourthly, this application provides a power module, including: a housing, components, a substrate, and a high-temperature resistant silicone gel as described in the third aspect above.
[0053] Both the substrate and the components are housed within the housing, with the components positioned on the surface of the substrate. High-temperature resistant silicone gel fills the gap between the substrate and the housing.
[0054] Optionally, the shell material includes at least one of glass fiber modified polyetheretherketone and carbon fiber modified polyetheretherketone.
[0055] Optionally, the component is a silicon carbide-based chip.
[0056] Fifthly, this application provides a method for preparing a power module as described in the fourth aspect above, comprising: pouring the composition as described in the first aspect above into a housing containing components and a substrate, and curing it at 110-130°C. Attached Figure Description
[0057] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of this application and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0058] Figure 1 A schematic diagram of the power module provided in this application is shown.
[0059] Figure 2 This paper presents a first-view structural schematic diagram of the components, substrate, and conductive terminals in the power module provided in this application.
[0060] Figure 3 This paper presents a second-view structural schematic diagram of the components, substrate, and conductive terminals in the power module provided in this application.
[0061] Figure 4 A schematic diagram of the components and substrate in the power module provided in this application is shown.
[0062] Figure 5 The diagram shows the penetration change curve of the silicone gel provided in Example 1 after aging at 250°C for 1000 hours.
[0063] Figure 6 The graph shows the change in penetration of the silicone gel provided in Example 2 after aging at 250°C for 1000 hours.
[0064] Figure 7 The graph shows the penetration change of the silicone gel provided in Example 3 after aging at 240°C for 1000 hours.
[0065] Figure 8 The graph shows the change in penetration of the silicone gel provided in Example 4 after aging at 230°C for 1000 hours.
[0066] Figure 9 The diagram shows the penetration change curve of the silicone gel provided in Example 5 after aging at 220°C for 1000 hours.
[0067] Labels: 100-Power Module; 110-Housing; 120-Components; 130-Substrate; 131-Copper Base Plate; 132-Ceramic Copper Clad Laminate; 1321-First Copper Layer; 1322-Second Copper Layer; 1323-First Region; 1324-Second Region; 1325-Third Region; 1326-Fourth Region; 133-Solder Layer; 140-Schottky Diode; 150-Wire; 151-First Aluminum Wire; 152-Second Aluminum Wire; 153-Third Aluminum Wire; 154-Fourth Aluminum Wire; 160-Conductive Terminal; 161-First Copper Terminal; 162-Second Copper Terminal; 163-Third Copper Terminal; 164-Fourth Copper Terminal. Detailed Implementation
[0068] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0069] This application provides a composition for preparing high-temperature resistant silicone gel, comprising: phenyl boron-containing vinyl silicone oil, phenyl-side hydrogen-containing silicone oil, platinum catalyst and inhibitor, wherein the mass ratio of phenyl boron-containing vinyl silicone oil, phenyl-side hydrogen-containing silicone oil, platinum catalyst and inhibitor is (10-20):(0.05-0.75):(0.06-0.4):(0.02-0.06).
[0070] The structural formula of phenyl boron-containing vinyl silicone oil is as follows:
[0071]
[0072] Where m and n are each an independent natural number greater than or equal to 1.
[0073] The structural formula of the phenyl-side hydrogen-containing silicone oil is as follows:
[0074]
[0075] In this context, x and y are each independent natural numbers greater than or equal to 1.
[0076] This application uses phenyl boron-containing vinyl silicone oil, phenyl-side hydrogen-containing silicone oil, platinum catalyst, and inhibitor, and adjusts the ratio of each component as a composition for preparing high-temperature resistant silicone gel. During the subsequent heating and curing process to prepare silicone gel, the inhibitor volatilizes and overflows from the system. Then, under the action of the platinum catalyst, the silicon-hydrogen bonds (-SiH) of the phenyl-side hydrogen-containing silicone oil break and undergo an addition curing reaction with the phenyl boron-containing vinyl silicone oil. This results in the silicone gel having both heat-resistant phenyl groups and high-bond-energy boron-oxygen bonds (BO) on the main chain, which is beneficial to improving the high-temperature resistance of the silicone gel.
[0077] As an example, the mass ratio of phenyl boron-containing vinyl silicone oil, phenyl-side hydrogen-containing silicone oil, platinum catalyst and inhibitor can be 10:0.05:0.06:0.02, 15:0.6:0.2:0.04 or 20:0.75:0.4:0.06, etc.
[0078] As an example, the phenyl boron-containing vinyl silicone oil with the above structure is prepared by the following method: Dimethyl dichlorosilane, benzene solvent, and deionized water are added to a three-necked flask and stirred mechanically at 25°C for 0.5-2 hours. After hydrolysis is completed, the acid-water mixture produced by hydrolysis is separated. A certain amount of phenylboronic acid and benzene solvent are then added to the hydrolysis product, and a certain amount of concentrated sulfuric acid is added as a catalyst. The temperature is raised to 50-70°C and the reaction is carried out for 3-7 hours. Divinyltetramethyldisiloxane is then added as a capping agent and the reaction is carried out for 1-2 hours. After the reaction is completed, the product is washed with water until neutral. Finally, the solvent and small molecules are removed by vacuum distillation to obtain colorless and transparent phenyl boron-containing vinyl silicone oil.
[0079] Furthermore, the benzene solvent includes at least one of toluene and xylene; the molar ratio of dimethyldichlorosilane to phenylboronic acid is (1-11):1; and the amount of concentrated sulfuric acid added is 3-10% of the total mass of the system.
[0080] It should be noted that the phenyl boron-containing vinyl silicone oil with the above structure can also be prepared by other methods, as long as the phenyl boron-containing vinyl silicone oil used meets the above structural requirements.
[0081] In this application, the molar ratio of silane hydride (-SiH) to silane vinyl group (-SiCH=CH2) in the composition is (1-1.5):1. This ratio is beneficial for further improving the high-temperature resistance and flexibility of the subsequently prepared silicone gel. If the content of silane vinyl group in the composition is too high, the silicone gel formed after addition curing will contain a large amount of unreacted silane vinyl group. Since silane vinyl group has poor stability at high temperatures, it will undergo thermo-oxidative degradation, leading to hardening of the silicone gel. If the content of silane hydride (-SiH) in the composition is too high, the reaction between the components will be insufficient, which is also detrimental to further improving the high-temperature resistance of the prepared silicone gel.
[0082] As an example, the inhibitor is selected from alkynyl alcohol inhibitors, including at least one of 1-ethynyl-1-cyclohexanol, 3,7,11-trimethyldodecyn-3-ol, 3,5-dimethyl-1-hexyn-3-ol, and 2-methyl-3-butyn-3-ol.
[0083] As an example, the molar ratio of silane-hydrogen group (-SiH) to silane-vinyl group (-SiCH=CH2) in the composition can be 1:1, 1:1.2, 1:1.3 or 1:1.5, etc.
[0084] Furthermore, the vinyl content in the boron-containing phenyl vinyl silicone oil is 0.28-0.32 mmol / g, the phenyl content in the boron-containing phenyl vinyl silicone oil is 8-30 mol%, the hydrogen content in the phenyl-side hydrogen-containing silicone oil is 1-8.5 mmol / g, and the phenyl content in the phenyl-side hydrogen-containing silicone oil is 30-50 mol%. Under these conditions, it is beneficial to further improve the high-temperature resistance and flexibility of the subsequently prepared silicone gel.
[0085] For example, the vinyl content in phenyl boron-containing vinyl silicone oil can be 0.28 mmol / g, 0.29 mmol / g, 0.30 mmol / g, or 0.32 mmol / g, etc., and the phenyl content in phenyl boron-containing vinyl silicone oil can be 8 mol%, 10 mol%, 15 mol%, 20 mol%, or 30 mol%, etc.; the hydrogen content in phenyl-side hydrogen-containing silicone oil can be 1 mmol / g, 3 mmol / g, 5 mmol / g, 7.5 mmol / g, or 8.5 mmol / g, etc., and the phenyl content in phenyl-side hydrogen-containing silicone oil can be 30 mol%, 32 mol%, 35 mol%, 45 mol%, or 50 mol%, etc.
[0086] As an example, the viscosity of phenyl boron-containing vinyl silicone oil is 800-2500 mPa·s, and the viscosity of phenyl-side hydrogen-containing silicone oil is 2.5-400 mPa·s.
[0087] In some feasible embodiments, the composition for preparing high-temperature resistant silicone gel further includes phenyl vinyl silicone oil; and the mass ratio of phenyl vinyl silicone oil to phenyl boron-containing vinyl silicone oil is (32.5-60):(10-20). In this case, it is advantageous to further improve the high-temperature resistance of the subsequently prepared silicone gel by increasing the phenyl content.
[0088] As an example, the mass ratio of phenyl vinyl silicone oil to phenyl boron-containing vinyl silicone oil can be 32.5:10, 40:15, or 60:20, etc.
[0089] Furthermore, the vinyl content in the phenyl vinyl silicone oil is 0.13-0.7 mmol / g; the phenyl content in the phenyl vinyl silicone oil is ≥35 mol%. Under these conditions, it is beneficial to further improve the high-temperature resistance of the subsequently prepared silicone gel.
[0090] For example, the vinyl content in phenyl vinyl silicone oil can be 0.13 mmol / g, 0.25 mmol / g, 0.5 mmol / g, 0.6 mmol / g, or 0.7 mmol / g, etc., and the phenyl content in phenyl vinyl silicone oil can be 35 mol%, 40 mol%, 45 mol%, or 50 mol%, etc.
[0091] As an example, the viscosity of phenyl vinyl silicone oil is 600-3000 mPa·s.
[0092] In some feasible embodiments, the composition for preparing high-temperature resistant silicone gel further includes phenyl-terminated hydrogen-containing silicone oil; and the mass ratio of phenyl-terminated hydrogen-containing silicone oil to phenyl-terminated hydrogen-containing silicone oil is (0.5-5):(0.05-0.75).
[0093] The structural formula of phenyl-terminated hydrogen-containing silicone oil is as follows:
[0094]
[0095] Where v and w are each an independent natural number greater than or equal to 1.
[0096] Adding the phenyl-terminated hydrogen-containing silicone oil in the above proportions helps to improve the toughness of the subsequently prepared silicone gel; it also helps to improve the adhesion performance of the subsequently prepared silicone gel. When the silicone gel is used to encapsulate power electronic components, it can improve the adhesion between the silicone gel and the power module shell and the components, thereby improving the structural stability of the power module.
[0097] As an example, the mass ratio of phenyl-terminated hydrogen-containing silicone oil to phenyl-side hydrogen-containing silicone oil can be 0.5:0.05, 2:0.5, or 5:0.75, etc.
[0098] Furthermore, the hydrogen content in the phenyl-terminated hydrogen-containing silicone oil is 3-6 mmol / g; the phenyl content in the phenyl-terminated hydrogen-containing silicone oil is 40-60 mol%. Under these conditions, it is beneficial to further improve the toughness and adhesive properties of the subsequently prepared silicone gel.
[0099] As an example, the hydrogen content in the phenyl-terminated hydrogen-containing silicone oil can be 3 mmol / g, 4 mmol / g, 4.5 mmol / g, or 6 mmol / g, etc., and the phenyl content in the phenyl-terminated hydrogen-containing silicone oil can be 40 mol%, 42 mol%, 45 mol%, 50 mol%, or 60 mol%, etc.
[0100] As an example, the viscosity of the phenyl-terminated hydrogen-containing silicone oil is 5-200 mPa·s.
[0101] In some feasible embodiments, the above-mentioned composition for preparing high-temperature resistant silicone gel further includes cage-type polysilsesquioxane; and the mass ratio of cage-type polysilsesquioxane to phenyl boron-containing vinyl silicone oil is (20-40):(10-20).
[0102] Cage-type polysilsesquioxane has a three-dimensional structure formed by a large number of Si-O-Si bonds. Adding cage-type polysilsesquioxane in the above ratio is beneficial to further improve the high temperature resistance of silica gel through a large number of inorganic Si-O bonds.
[0103] As an example, the mass ratio of cage-type polysilsesquioxane to phenyl boron-containing vinyl silicone oil can be 20:10, 25:20, or 40:10, etc.
[0104] As an example, the cage-type polysilsesquioxane is selected from glycidyl-cage-type polysilsesquioxane, and the viscosity of the cage-type polysilsesquioxane is 3500-4800 mPa·s.
[0105] In some feasible embodiments, the above-mentioned composition for preparing high-temperature resistant silicone gel further includes a heat resistant agent, which includes rare earth metal complexes; and the mass ratio of the heat resistant agent to phenyl boron-containing vinyl silicone oil is (1-5):(10-20).
[0106] Using rare earth metal complexes as heat-resistant agents, the introduction of rare earth metal complexes in the above-mentioned proportions will not affect the transparency of the silicone gel. At the same time, rare earth metal complexes can prevent free radical reactions caused by oxidation in the silicone gel at high temperatures, can be regenerated under the action of oxygen in the air, and can also play a role in thermal stability of the silicone gel by absorbing some acidic or alkaline substances in the silicone gel that can catalyze degradation reactions. This achieves the purpose of preventing the oxidative crosslinking of polysiloxane side chains and the cyclization degradation of the main chain, which is beneficial to extending the service life of silicone gel at high temperatures.
[0107] As an example, the mass ratio of the heat resistant agent to the phenyl boron-containing vinyl silicone oil can be 1:10, 2:15, or 5:20, etc.
[0108] As an example, the rare earth metal complex selected as the heat-resistant agent can be a transparent nano-dispersion of cerium oxide rare earth complex.
[0109] This application also provides a method for preparing high-temperature resistant silicone gel, comprising: curing the above-provided composition for preparing high-temperature resistant silicone gel at 110-130°C.
[0110] The silicone gel prepared by the above method has excellent high temperature resistance and can be used as a silicone gel for packaging high-power electronic components such as SiC-based devices to meet the needs of high-power modules that generate a lot of heat and need to work at high temperatures for a long time.
[0111] Understandably, the components in the composition used to prepare the high-temperature resistant silicone gel are in a mixed state before curing.
[0112] For example, the curing temperature can be 110℃, 115℃, 120℃, 125℃, or 130℃, etc. The curing time can be 0.5-1h.
[0113] In the embodiments of this application, before curing, the method for preparing the composition for preparing high-temperature resistant silicone gel includes: mixing a first raw material and a second raw material under vacuum; wherein, the first raw material includes, by weight, 20-40 parts of phenyl boron-containing vinyl silicone oil and 0.12-0.8 parts of platinum catalyst; the second raw material includes, by weight, 0.1-1.5 parts of phenyl-side hydrogen-containing silicone oil and 0.04-0.12 parts of inhibitor.
[0114] Preparing the pre-cured composition by mixing the first and second raw materials under vacuum conditions helps avoid the increase in viscosity that can occur when directly mixing all components before heating and curing begins, which leads to an addition curing reaction between some phenyl-side hydrogen-containing silicone oil and some phenyl-side boron-containing vinyl silicone oil. When the composition is poured into the power module housing, a high viscosity not only hinders pouring but also results in air bubbles inside the housing after pouring, leading to poor encapsulation.
[0115] Furthermore, the first raw material also includes 60-80 parts by weight of phenyl vinyl silicone oil.
[0116] Furthermore, the second raw material also includes 5-40 parts by weight of phenyl vinyl silicone oil.
[0117] Optionally, the second raw material further includes 1-10 parts by weight of phenyl-terminated hydrogen-containing silicone oil; the structural formula of the phenyl-terminated hydrogen-containing silicone oil is as follows:
[0118]
[0119] Where v and w are each an independent natural number greater than or equal to 1.
[0120] Optionally, the second raw material may also include 40-80 parts by weight of cage-type polysilsesquioxane.
[0121] Optionally, the second raw material may also include 2-10 parts by weight of a heat-resistant agent; the heat-resistant agent may include rare earth metal complexes.
[0122] In the embodiments of this application, the step of mixing the first raw material and the second raw material includes: mixing and stirring the first raw material and the second raw material at a speed of 1200-1800 rpm for 120-180 seconds.
[0123] As an example, the vacuum degree of the mixture of the first raw material and the second raw material is -0.99 kPa.
[0124] This application also provides a high-temperature resistant silicone gel, which is prepared by the above-described method for preparing high-temperature resistant silicone gel.
[0125] The high-temperature resistant silicone gel provided in this application has excellent high-temperature resistance and can be used as a silicone gel for encapsulating high-power electronic components such as SiC-based devices to meet the needs of high-power modules that generate a lot of heat and need to operate at high temperatures for a long time.
[0126] Figure 1 A schematic diagram of the power module 100 provided in this application is shown. Figure 2This is a first-view structural schematic diagram of the components 120, substrate 130, and conductive terminals 160 in the power module 100 provided in this application. Figure 3 This is a second-view structural schematic diagram of the components 120, substrate 130, and conductive terminals 160 in the power module 100 provided in this application. Figure 4 This paper shows a schematic diagram of the structure of components 120 and substrate 130 in the power module 100 provided in this application. Please refer to [link / reference]. Figures 1 to 4 This application also provides a power module 100, including: a housing 110, components 120, a substrate 130, and high-temperature resistant silicone gel (not shown in the figure) as described above. The substrate 130 and components 120 are both disposed within the housing 110, and the components 120 are disposed on the surface of the substrate 130. The high-temperature resistant silicone gel fills the gap between the substrate 130 and the housing 110.
[0127] In this application, the material of the housing 110 includes at least one of glass fiber modified polyetheretherketone (PEEK) and carbon fiber modified PEEK; the component 120 is a silicon carbide MOS chip. Using the aforementioned materials for the housing 110 improves its high-temperature resistance, and when combined with the high-temperature resistant silicone gel provided in this application, it further enhances the overall high-temperature resistance of the power module 100.
[0128] Component 120 has a source, a gate, a drain, and a Kelvin source portion.
[0129] The substrate 130 includes a copper base plate 131, a ceramic copper-clad laminate 132, and a solder layer 133 connecting the copper base plate 131 and the ceramic copper-clad laminate 132. The ceramic copper-clad laminate 132 has a first copper layer 1321 on the side near the copper base plate 131 and a second copper layer 1322 on the side away from the copper base plate 131. The second copper layer 1322 includes a first region 1323 (for connecting the gate portion), a second region 1324 (for connecting the drain portion), a third region 1325 (for connecting the Kelvin source portion), and a fourth region 1326 (for connecting the source portion), spaced apart from each other. A component 120 is disposed on the second region 1324. A Schottky diode 140 is also disposed on the second region 1324.
[0130] The power module 100 also has aluminum wires 150, which include a first aluminum wire 151 connecting the first region 1323 and the gate of the component 120, a second aluminum wire 152 connecting the fourth region 1326 and the source of the component 120, a third aluminum wire 153 connecting the third region 1325 and the Kelvin source of the component 120, and a fourth aluminum wire 154 connecting the fourth region 1326 and the Schottky diode 140.
[0131] Furthermore, the power module 100 also includes conductive terminals 160 extending from the housing 110. The conductive terminals 160 include a first copper terminal 161 for connecting to the gate of the MOS, a second copper terminal 162 for connecting to the drain of the MOS, a third copper terminal 163 for connecting to the Kelvin source of the MOS, and a fourth copper terminal 164 for connecting to the source of the MOS.
[0132] This application also provides a method for preparing a power module 100, which includes pouring the composition for preparing high-temperature resistant silicone gel as described above into a housing 110 containing components 120 and a substrate 130, and curing it at 110-130°C.
[0133] Furthermore, before infusion, the first and second raw materials mentioned above are mixed under vacuum to form a composition, and then the composition is immediately infused into the housing 110 containing the components 120 and the substrate 130, and then immediately cured at 110-130°C.
[0134] As an example, before potting, the steps of preparing the housing 110 containing the components 120 and the substrate 130 include: firstly, soldering the ceramic copper-clad laminate 132 (including the first copper layer 1321, the intermediate alumina ceramic and the second copper layer 1322) onto the copper base plate 131 with solder (i.e., soldering the first copper layer 1321 to the copper base plate 131) to obtain the substrate 130; secondly, soldering the SiC-based chip (i.e., the components 120) and the Schottky diode 140 to the surface of the second copper layer 1322 of the substrate 130 with solder; then connecting the surface of the components 120 and the surface of the Schottky diode 140 to the second copper layer 1322 of the substrate 130 with wires 150; finally, adding a plastic housing 110 of glass fiber or carbon fiber modified PEEK and leading out conductive terminals 160 to the outside of the housing 110.
[0135] The features and properties of the high-temperature resistant silicone gel of this application are further described in detail below with reference to the embodiments.
[0136] Example 1
[0137] This embodiment provides a high-temperature resistant silica gel, which is prepared using the following method:
[0138] (1) By weight, 70 parts of phenyl vinyl silicone oil, 29.5 parts of phenyl boron-containing vinyl silicone oil and 0.5 parts of platinum catalyst were stirred and mixed for 150s under a vacuum of -0.99Kpa and a speed of 1500rpm to obtain the first raw material.
[0139] Among them, the phenyl vinyl silicone oil has a vinyl content of 0.5 mmol / g and a phenyl content of 40 mol%, and a viscosity of 1000 mPa·s; the phenyl boron-containing vinyl silicone oil has a vinyl content of 0.3 mmol / g and a phenyl content of 15 mol%, and a viscosity of 1200 mPa·s.
[0140] (2) By weight, 33.4 parts of phenyl vinyl silicone oil, 1.5 parts of phenyl-side hydrogen-containing silicone oil, 10 parts of phenyl-terminated hydrogen-containing silicone oil, 50 parts of glycidyl-cage polysilsesquioxane, 0.1 parts of 1-ethynyl-1-cyclohexanol and 5 parts of cerium oxide organosilicon dispersion were stirred and mixed for 150s under a vacuum of -0.99Kpa and a speed of 1500rpm to obtain the second raw material.
[0141] Among them, the phenyl vinyl silicone oil has a vinyl content of 0.5 mmol / g and a phenyl content of 40 mol%, and its viscosity is 1000 mPa·s; the phenyl-side hydrogen-containing silicone oil has a hydrogen content of 5 mmol / g and a phenyl content of 45 mol%, and its viscosity is 200 mPa·s; the phenyl-terminated hydrogen-containing silicone oil has a hydrogen content of 5 mmol / g and a phenyl content of 50 mol%, and its viscosity is 100 mPa·s; and the glycidyl-cage-type polysilsesquioxane has a viscosity of 4000 mPa·s.
[0142] (3) The first raw material obtained in step (1) and the second raw material obtained in step (2) are mixed at a mass ratio of 1:1 and stirred for 150s at a vacuum of -0.99Kpa and a speed of 1500rpm; then cured at 120℃ for 1h to obtain high temperature resistant silicone gel.
[0143] Example 2
[0144] This embodiment provides a high-temperature resistant silicone gel. The preparation steps of this embodiment are largely the same as those of Example 1, except that the second raw material in this embodiment does not contain phenyl-terminated hydrogen-containing silicone oil. Step (2) of this embodiment is as follows:
[0145] By weight, 33.4 parts of phenyl vinyl silicone oil, 11.5 parts of phenyl-side hydrogen silicone oil, 50 parts of glycidyl-cage polysilsesquioxane, 0.1 parts of 1-ethynyl-1-cyclohexanol, and 5 parts of cerium oxide organosilicon dispersion were stirred and mixed for 150 s under a vacuum of -0.99 kPa and a speed of 1500 rpm to obtain the second raw material.
[0146] Example 3
[0147] This embodiment provides a high-temperature resistant silicone gel. The preparation steps of this embodiment are largely the same as those of Example 1, except that the second raw material in this embodiment does not contain glycidyl-cage-type polysilsesquioxane. Step (2) of this embodiment is as follows:
[0148] By weight, 83.4 parts of phenyl vinyl silicone oil, 1.5 parts of phenyl-side hydrogen-containing silicone oil, 10 parts of phenyl-terminated hydrogen-containing silicone oil, 0.1 parts of 1-ethynyl-1-cyclohexanol, and 5 parts of cerium oxide organosilicon dispersion were stirred and mixed for 150 s under a vacuum of -0.99 kPa and a speed of 1500 rpm to obtain the second raw material.
[0149] Example 4
[0150] This embodiment provides a high-temperature resistant silicone gel. The preparation steps of this embodiment are largely the same as those of Example 1, except that the second raw material in this embodiment does not contain cerium oxide organosilicon dispersion. Step (2) of this embodiment is as follows:
[0151] By weight, 38.4 parts of phenyl vinyl silicone oil, 1.5 parts of phenyl-side hydrogen-containing silicone oil, 10 parts of phenyl-terminated hydrogen-containing silicone oil, 50 parts of glycidyl-cage-type polysilsesquioxane, and 0.1 parts of 1-ethynyl-1-cyclohexanol were stirred and mixed for 150 s under a vacuum of -0.99 kPa and a speed of 1500 rpm to obtain the second raw material.
[0152] Example 5
[0153] This embodiment provides a high-temperature resistant silica gel, which is prepared using the following method:
[0154] (1) Phenyl boron vinyl silicone oil, platinum catalyst, phenyl hydrogen silicone oil and 1-ethynyl-1-cyclohexanol in a mass ratio of 29.5:0.5:1.5:0.1 were stirred and mixed for 150s under a vacuum of -0.99Kpa and a speed of 1500rpm to obtain a composition for preparing high-temperature resistant silicone gel.
[0155] Among them, the phenyl boron-containing vinyl silicone oil has a vinyl content of 0.3 mmol / g and a phenyl content of 15 mol%, and a viscosity of 1200 mPa·s; the phenyl-side hydrogen-containing silicone oil has a hydrogen content of 5 mmol / g and a phenyl content of 45 mol%, and a viscosity of 200 mPa·s.
[0156] (2) The composition obtained in step (1) is cured at 120°C for 1 hour to obtain a high-temperature resistant silicone gel.
[0157] Comparative Example 1
[0158] This comparative example provides a silicone gel. The preparation steps of this comparative example are largely the same as those of Example 1, except that the first raw material in this comparative example does not contain phenyl boron-containing vinyl silicone oil. Step (1) of this example is as follows:
[0159] By weight, 99.5 parts of phenyl vinyl silicone oil and 0.5 parts of platinum catalyst were stirred and mixed for 150 seconds under a vacuum of -0.99 kPa and a speed of 1500 rpm to obtain the first raw material.
[0160] Comparative Example 2
[0161] This comparative example provides a silicone gel. The preparation steps of this comparative example are largely the same as those of Example 1, except that the first raw material in this comparative example does not contain phenyl-side hydrogen-containing silicone oil. Step (2) of this example is as follows:
[0162] By weight, 34.9 parts of phenyl vinyl silicone oil, 10 parts of phenyl-terminated hydrogen silicone oil, 50 parts of glycidyl-cage-type polysilsesquioxane, 0.1 parts of 1-ethynyl-1-cyclohexanol, and 5 parts of cerium oxide organosilicon dispersion were stirred and mixed for 150 s under a vacuum of -0.99 kPa and a speed of 1500 rpm to obtain the second raw material.
[0163] Experimental Example
[0164] The performance of the silicone gels provided in Examples 1-5 and Comparative Examples 1-2 was characterized, and the results are shown in Table 1. The penetration change of the silicone gels provided in Examples 1-5 after aging at the highest long-term operating temperature for 1000 hours was tested, and the results are shown below. Figure 5-9 As shown; Figures 5 to 9 Penetration refers to the depth of penetration. Figures 5 to 9 The test temperatures were 250℃, 250℃, 240℃, 230℃, and 220℃.
[0165] Table 1
[0166]
[0167] In Table 1, the maximum long-term withstand temperature is defined as the temperature at which the silicone gel undergoes a 1000-hour aging process at a constant temperature. After 1000 hours, the penetration rate of the silicone gel changes by ≤15%, and the penetration rate drops rapidly to 0 at any point within 1000 hours of aging at any temperature exceeding this constant temperature (after which it can no longer be tested with a penetration tester). "-" indicates that the corresponding data cannot be measured.
[0168] As shown in Table 1, the highest long-term endurance temperature of the silicone gels prepared in Examples 1-5 is higher than that of the silicone gel prepared in Comparative Example 1. This indicates that, compared to Comparative Example 1 which does not use phenyl boron-containing vinyl silicone oil, using phenyl boron-containing vinyl silicone oil in the raw materials for preparing the silicone gels in Examples 1-5 can effectively improve the high-temperature resistance of the prepared silicone gels. However, Comparative Example 2, because it did not use phenyl-side hydrogen-containing silicone oil, could not be cured and formed into a silicone gel.
[0169] Furthermore, a comparison between Example 1 and Example 2 reveals that the difference lies in the following: Example 1 uses 1.5 parts of phenyl-side hydrogen-containing silicone oil and 10 parts of phenyl-terminated hydrogen-containing silicone oil, while Example 2 uses 11.5 parts of phenyl-side hydrogen-containing silicone oil (i.e., no phenyl-side hydrogen-containing silicone oil). The elongation at break (reflecting toughness) and shear strength (reflecting adhesion performance) of the silicone gel prepared in Example 2 are both inferior to those prepared in Example 1. This indicates that when the phenyl content in the raw materials for preparing the silicone gel is consistent, using phenyl-terminated hydrogen-containing silicone oil can improve the toughness and adhesion performance of the prepared silicone gel.
[0170] A comparison between Example 1 and Example 3 shows that the difference between Example 1 and Example 3 is that Example 3 does not contain glycidyl-cage polysilsesquioxane, and the maximum long-term endurance temperature of the silicone gel prepared in Example 3 is slightly lower than that of the silicone gel prepared in Example 1. This indicates that the addition of glycidyl-cage polysilsesquioxane can help to further improve the high-temperature resistance of the prepared silicone gel.
[0171] A comparison between Example 1 and Example 4 shows that the difference between Example 1 and Example 4 is that Example 4 does not contain cerium oxide organosilicon dispersion (i.e., heat resistant agent), and the maximum long-term endurance temperature of the silicone gel prepared in Example 4 is slightly lower than that of the silicone gel prepared in Example 1. This indicates that the addition of cerium oxide organosilicon dispersion can help to further improve the high-temperature resistance of the prepared silicone gel.
[0172] The difference between Example 1 and Example 5 is that Example 5 contains only phenyl boron-containing vinyl silicone oil, platinum catalyst, phenyl-side hydrogen-containing silicone oil, and 1-ethynyl-1-cyclohexanol, but does not contain phenyl vinyl silicone oil, phenyl-terminated hydrogen-containing silicone oil, glycidyl-cage polysilsesquioxane, or cerium oxide organosilicon dispersion. A comparison of Example 1, Comparative Example 1, and Example 5 shows that the highest long-term endurance temperature of the silicone gel prepared in Example 5 is lower than that of the silicone gel prepared in Example 1, but higher than that of the silicone gel prepared in Comparative Example 1. This indicates that the combination of phenyl boron-containing vinyl silicone oil and phenyl-side hydrogen-containing silicone oil can effectively improve the high-temperature resistance of the prepared silicone gel.
[0173] from Figure 5-9 It can be seen that the silicone gels prepared in Examples 1-5 are stable at 250℃, 250℃, 240℃, 230℃, 220℃ and 200℃ respectively. After aging at 250℃, 250℃, 240℃, 230℃ and 220℃ for 1000h respectively, the change in penetration value of the silicone gels prepared in Examples 1-5 is not significant. This indicates that the silicone gels prepared in Examples 1-5 of this application are not prone to hardening or cracking due to long-term use at high temperature.
[0174] In summary, the high-temperature resistant silicone gel provided in this application, during the subsequent heating and curing process to prepare silicone gel, results in the formation of silicone gel with both heat-resistant phenyl groups and high-bond-energy boron-oxygen bonds (BO) on the main chain, which is beneficial to improving the high-temperature resistance of the silicone gel.
[0175] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A composition for preparing high-temperature resistant silica gel, characterized in that, include: Phenyl boron-containing vinyl silicone oil, phenyl-side hydrogen-containing silicone oil, platinum catalyst and inhibitor; The mass ratio of the phenyl boron-containing vinyl silicone oil, the phenyl-side hydrogen-containing silicone oil, the platinum catalyst, and the inhibitor is (10-20):(0.05-0.75):(0.06-0.4):(0.02-0.06). The structural formula of the phenyl boron-containing vinyl silicone oil is as follows: ; Where m and n are each an independent natural number greater than or equal to 1; The structural formula of the phenyl-side hydrogen-containing silicone oil is as follows: ; In this case, x and y are each independent natural numbers greater than or equal to 1.
2. The composition according to claim 1, characterized in that, The molar ratio of silane groups to silane vinyl groups in the composition is (1-1.5):1; The phenyl boron-containing vinyl silicone oil contains 0.28-0.32 mmol / g of vinyl groups; the phenyl content in the phenyl boron-containing vinyl silicone oil is 8-30 mol%. The hydrogen content in the phenyl-side hydrogen-containing silicone oil is 1-8.5 mmol / g; the phenyl content in the phenyl-side hydrogen-containing silicone oil is 30-50 mol% The viscosity of the phenyl boron-containing vinyl silicone oil is 800-2500 mPa·s; The viscosity of the phenyl-side hydrogen-containing silicone oil is 2.5-400 mPa·s.
3. The composition according to claim 1, characterized in that, The composition further includes phenyl vinyl silicone oil; the mass ratio of the phenyl vinyl silicone oil to the phenyl boron-containing vinyl silicone oil is (32.5-60):(10-20); The vinyl content in the phenyl vinyl silicone oil is 0.13-0.7 mmol / g; the phenyl content in the phenyl vinyl silicone oil is ≥35 mol% The viscosity of the phenyl vinyl silicone oil is 600-3000 mPa·s.
4. The composition according to claim 1, characterized in that, The composition further includes a phenyl-terminated hydrogen-containing silicone oil; the mass ratio of the phenyl-terminated hydrogen-containing silicone oil to the phenyl-terminated hydrogen-containing silicone oil is (0.5-5):(0.05-0.75). The structural formula of the phenyl-terminated hydrogen-containing silicone oil is as follows: ; Where v and w are each an independent natural number greater than or equal to 1; The hydrogen content in the phenyl-terminated hydrogen-containing silicone oil is 3-6 mmol / g; the phenyl content in the phenyl-terminated hydrogen-containing silicone oil is 40-60 mol% The viscosity of the phenyl-terminated hydrogen-containing silicone oil is 5-200 mPa·s.
5. The composition according to claim 1, characterized in that, The composition further includes cage-type polysilsesquioxane; the mass ratio of the cage-type polysilsesquioxane to the phenyl boron-containing vinyl silicone oil is (20-40):(10-20); The cage-type polysilsesquioxane is a glycidyl-cage-type polysilsesquioxane; The viscosity of the cage-type polysilsesquioxane is 3500-4800 mPa·s.
6. The composition according to claim 1, characterized in that, The composition further includes a heat resistant agent; the mass ratio of the heat resistant agent to the phenyl boron-containing vinyl silicone oil is (1-5):(10-20); The heat-resistant agent is a cerium oxide organosilicon dispersion; The inhibitor is selected from alkynol inhibitors, which include at least one of 1-ethynyl-1-cyclohexanol, 3,7,11-trimethyldodecyn-3-ol, 3,5-dimethyl-1-hexyn-3-ol, and 2-methyl-3-butyn-3-ol.
7. A method for preparing a high-temperature resistant silica gel, characterized in that, include: The composition as described in claim 1 is cured at 110-130°C.
8. The preparation method according to claim 7, characterized in that, The method for preparing the composition includes: mixing a first raw material and a second raw material under vacuum conditions; wherein, the first raw material comprises, by weight, 20-40 parts of the phenyl boron-containing vinyl silicone oil and 0.12-0.8 parts of the platinum catalyst; the second raw material comprises, by weight, 0.1-1.5 parts of the phenyl-side hydrogen-containing silicone oil and 0.04-0.12 parts of the inhibitor; The first raw material also includes 60-80 parts by weight of phenyl vinyl silicone oil; The second raw material also includes 5-40 parts by weight of phenyl vinyl silicone oil; The second raw material further includes 1-10 parts by weight of phenyl-terminated hydrogen-containing silicone oil; the structural formula of the phenyl-terminated hydrogen-containing silicone oil is as follows: ; Where v and w are each an independent natural number greater than or equal to 1; The second raw material also includes 40-80 parts by weight of cage-type polysilsesquioxane; The second raw material also includes 2-10 parts by weight of a heat-resistant agent; the heat-resistant agent is a rare earth metal complex.
9. A high-temperature resistant silicone gel, characterized in that, The high-temperature resistant silica gel is prepared by the method described in claim 7.
10. A power module, characterized in that, include: The housing, components, substrate, and the high-temperature resistant silicone gel as described in claim 9.
11. The power module according to claim 10, characterized in that, Both the substrate and the components are disposed within the housing, and the components are disposed on the surface of the substrate. The high-temperature resistant silicone gel fills the gap between the substrate and the housing. The material of the outer shell includes at least one of glass fiber modified polyetheretherketone and carbon fiber modified polyetheretherketone; The component is a silicon carbide-based chip.
12. A method for preparing a power module as described in claim 10, characterized in that, include: The composition as described in claim 1 is poured into the housing containing the components and the substrate, and cured at 110-130°C.
Citation Information
Patent Citations
Silica gel for electronic components and preparation method thereof
CN103709988A
High-heat-conductivity boroheteropolysiloxane potting adhesive and preparation method thereof
CN104031603A