A water-resistant and anti-fouling water-based environmentally friendly ink and preparation method thereof

By using water-resistant and anti-fouling resin and specific process treatment in water-based ink, the problem of poor water resistance of water-based ink when tipping paper gets damp is solved, achieving better adhesion fastness and anti-fouling effect, and improving the appearance of printed products. performance and durability.

CN117701066BActive Publication Date: 2024-10-29SHENZHEN FANG RUN ENVIRONMENTAL TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311792318.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-25
Publication Date
2024-10-29
Estimated Expiration
2043-12-25

AI Technical Summary

Technical Problem

Existing water-based inks have poor water resistance when tipping paper gets damp or soaked in water, and their adhesion fastness and tinting power drop sharply. They are prone to stains and affect the aesthetics of printed products.

Method used

Water-resistant and anti-fouling resin, ethanol and deionized water are used to stir and mix, and pigments, polyethylene wax, titanium dioxide and DC-65 defoaming agent are added to prepare water-resistant and anti-fouling water-based environmentally friendly ink through specific process steps to form a carbon-containing The molecular structure of chains, benzene rings and C-F bonds improves the water resistance and antifouling properties of the ink.

Benefits of technology

Significantly improves the water resistance and antifouling performance of the ink, avoids stains, and maintains the aesthetics and service life of printed products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004626717940000021
    Figure BDA0004626717940000021
  • Figure BDA0004626717940000031
    Figure BDA0004626717940000031
  • Figure BDA0004626717940000032
    Figure BDA0004626717940000032
Patent Text Reader

Abstract

The invention relates to the field of inks, and in particular to a water-resistant and antifouling water-based environmentally friendly ink and a preparation method thereof, which are used to solve the problems that the existing water-based inks still have poor water resistance, poor hydrolysis resistance when tipping paper is damp or soaked in water, sharp decreases in adhesion fastness and tinting strength, and are easily stained, thus affecting the aesthetics of printed products; the molecular structure of the water-resistant and antifouling resin contains a carbon chain to give it good flexibility, and a large number of benzene rings to give it good rigidity and stability, making it difficult to be destroyed, and the water-resistant and antifouling resin also contains a large number of C-F bonds, which have large bond energy and good stability and are difficult to be destroyed, and can reduce its surface energy, showing good hydrophobicity, thereby improving its water resistance, and can also show excellent waterproof and oil-proof effects, avoid staining, and achieve anti-fouling effect, therefore, the environmentally friendly ink using the water-resistant and antifouling resin as a main raw material has good water resistance and anti-fouling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of inks, and in particular to a water-resistant and anti-fouling water-based environmentally friendly ink and a preparation method thereof. Background Art

[0002] Water-based ink uses water as the main solvent, with almost no volatile organic compound (VOC) emissions and no pollution to the atmosphere. Water is the cheapest solvent, so the manufacturing cost of water-based ink is lower than any other type of printing ink, which has the advantage of low cost. The manufacturing environment of water-based ink is safe, which protects the health of operators, reduces resource consumption, and reduces environmental protection costs. Water-based ink printing can reduce or even eliminate organic residues in printed products, ensuring the health and safety of users.

[0003] However, the water-based ink currently used still has poor water resistance. When the tipping paper is damp or soaked in water, the hydrolysis resistance is poor, the adhesion fastness and coloring strength drop sharply, and it is easy to be stained, affecting the aesthetics of the printed product. Summary of the invention

[0004] In order to overcome the above-mentioned technical problems, the purpose of the present invention is to provide a water-resistant and anti-fouling water-based environmentally friendly ink and a preparation method thereof: by adding a water-resistant and anti-fouling resin, ethanol and deionized water into a mixer and stirring and mixing, and then adding a pigment, polyethylene wax, titanium dioxide and DC-65 defoaming agent and continuing to stir and mix, the water-resistant and anti-fouling water-based environmentally friendly ink is obtained, which solves the problems that the existing water-based ink still has poor water resistance, poor hydrolysis resistance when the tipping paper is damp or soaked in water, a sharp decrease in adhesion fastness and tinting strength, and is easy to be stained, affecting the aesthetics of the printed product.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for preparing a water-resistant and anti-fouling water-based environmentally friendly ink comprises the following steps:

[0007] Step 1: Weigh 50-70 parts of water-resistant and antifouling resin, 8-15 parts of pigment, 2-7 parts of polyethylene wax, 4-8 parts of titanium dioxide, 0.8-1.4 parts of DC-65 defoamer, 12-20 parts of ethanol and 20-30 parts of deionized water according to weight parts, and set aside;

[0008] Step 2: Add the water-resistant and antifouling resin, ethanol and deionized water into a mixer, stir and mix for 1-2 hours at a stirring rate of 1000-1500r / min, then add the pigment, polyethylene wax, titanium dioxide and DC-65 defoaming agent and continue stirring and mixing for 2-3 hours to obtain the water-resistant and antifouling water-based environmentally friendly ink.

[0009] As a further solution of the present invention: the water-resistant and antifouling resin is prepared by the following steps:

[0010] Step s1: add biphenyl, paraformaldehyde, concentrated hydrochloric acid, glacial acetic acid, zinc chloride and cyclohexane into a three-necked flask equipped with a thermometer, a stirrer and an air duct, stir and react for 30-40 minutes at a temperature of 35-40°C and a stirring rate of 400-500r / min, then heat to 45-50°C and introduce hydrogen chloride gas while stirring until the reaction system is saturated, then stir and react at a constant temperature for 6-8 hours, after the reaction is completed, cool the reaction product to room temperature, then add it to distilled water, then stand and stratify, remove the water layer, then wash with distilled water until neutral, then cool to below 0°C, precipitate, then vacuum filter, place the filter cake in a vacuum drying oven, and dry it at a temperature of 90-95°C for 2-3 hours to obtain intermediate 1;

[0011] The reaction process is as follows:

[0012]

[0013] Step s2: Add intermediate 1, 3,5-dimethoxyphenol, anhydrous potassium carbonate, N,N-dimethylacetamide and toluene into a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir and react for 20-30 minutes at a temperature of 25-30° C. and a stirring rate of 400-500 r / min, then heat to 140-145° C. and continue stirring and reacting for 10-15 hours. After the reaction is completed, cool the reaction product to room temperature, then add it to distilled water, precipitate, vacuum filter, wash the filter cake with distilled water 3-5 times, and then recrystallize with a mixed solvent to obtain intermediate 2;

[0014] The reaction process is as follows:

[0015]

[0016] Step s3: Add intermediate 2 and dichloromethane to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, add boron tribromide solution dropwise while stirring at a temperature of -10°C and a stirring rate of 400-500 r / min, and control the dropping rate to 1-2 drops / s. After the dropwise addition is completed, continue stirring and react for 6-8 hours. After the reaction is completed, add the reaction product to a saturated sodium bicarbonate solution, then vacuum filter, wash the filter cake with distilled water 3-5 times, and then recrystallize with an ethanol solution to obtain intermediate 3;

[0017] The reaction process is as follows:

[0018]

[0019] Step s4: Add intermediate 3, anhydrous potassium carbonate, N,N-dimethylacetamide and toluene into a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir and react for 1-2 hours at a temperature of 140-150° C. and a stirring rate of 400-500 r / min, then add 2-chloro-5-nitrotrifluorotoluene and continue stirring and reacting for 10-15 hours. After the reaction is completed, the reaction product is cooled to room temperature, then added into distilled water, precipitated, vacuum filtered, and the filter cake is washed with distilled water for 3-5 times, then placed in a vacuum drying oven, and dried at a temperature of 80-85° C. for 3-5 hours to obtain intermediate 4;

[0020] The reaction process is as follows:

[0021]

[0022] Step s5: Add intermediate 4, 10% palladium carbon and anhydrous ethanol to a four-necked flask equipped with a thermometer, a stirrer, an air guide tube, a constant pressure dropping funnel and a reflux condenser, introduce nitrogen protection, stir the reaction for 10-15 minutes at a temperature of 25-30°C and a stirring rate of 400-500r / min, then heat the mixture to reflux and add hydrazine hydrate solution dropwise while stirring, control the dropping rate to 1-2 drops / s, continue stirring the reaction for 8-10 hours after the dropwise addition is completed, and cool the reaction product to room temperature after the reaction is completed, then vacuum filter, and rotary evaporate the filtrate to remove the solvent to obtain intermediate 5;

[0023] The reaction process is as follows:

[0024]

[0025] Step s6: Add intermediate 5, propylene carbonate and chloroform into a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, introduce nitrogen protection, stir at a stirring rate of 400-500 r / min while heating to reflux, and continue stirring and reacting for 4-5 hours, and control the heating rate to 2-4°C / min. After the reaction, cool the reaction product to room temperature, then rotary evaporate to remove the solvent, and then recrystallize with anhydrous ethanol to obtain intermediate 6;

[0026] The reaction process is as follows:

[0027]

[0028] Step s7: Add intermediate 6, diphenylmethane diisocyanate, dibutyltin dilaurate and N,N-dimethylformamide to a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir the reaction at a temperature of 40-45°C and a stirring rate of 400-500r / min for 1-2h, then raise the temperature to 85-90°C and continue stirring the reaction for 4-5h. After the reaction is completed, the reaction product is cooled to room temperature, then placed in a vacuum drying oven, and dried at a temperature of 60-65°C for 8-10h to obtain a water-resistant and anti-fouling resin.

[0029] The reaction process is as follows:

[0030]

[0031] As a further solution of the present invention: the pigment in step 1 is one or a mixture of two or more of benzidine yellow G, litho scarlet, phthalocyanine blue, phthalocyanine green, phthalocyanine violet and carbon black in any proportion.

[0032] As a further solution of the present invention: the usage ratio of the biphenyl, paraformaldehyde, concentrated hydrochloric acid, glacial acetic acid, zinc chloride and cyclohexane in step s1 is 0.1 mol: 7-8 g: 8-10 mL: 25-30 mL: 0.2-0.25 mol: 80-100 mL, and the mass fraction of the concentrated hydrochloric acid is 36-38%.

[0033] As a further scheme of the present invention: the usage ratio of the intermediate 1, 3,5-dimethoxyphenol, anhydrous potassium carbonate, N,N-dimethylacetamide and toluene in step s2 is 0.1 mol: 0.2 mol: 0.22-0.25 mol: 120-150 mL: 50-60 mL, and the mixed solvent is an equal volume mixture of anhydrous ethanol and acetone.

[0034] As a further solution of the present invention: the dosage ratio of the intermediate 2, dichloromethane and boron tribromide solution in step s3 is 10 mmol: 20-25 mL: 80-100 mL, the boron tribromide solution is a 1-1.2 mol / L solution formed by dissolving boron tribromide in dichloromethane, and the volume fraction of the ethanol solution is 70-80%.

[0035] As a further scheme of the present invention: the usage ratio of the intermediate 3, anhydrous potassium carbonate, N,N-dimethylacetamide, toluene and 2-chloro-5-nitrotrifluorotoluene in step s4 is 10 mmol:45-50 mmol:120-150 mL:50-60 mL:40 mmol.

[0036] As a further solution of the present invention: the usage ratio of the intermediate 4, 10% palladium carbon, anhydrous ethanol and hydrazine hydrate solution in step s5 is 10 mmol: 0.2-0.3 g: 100-120 mL: 15-20 mL, and the mass fraction of the hydrazine hydrate solution is 50-60%.

[0037] As a further solution of the present invention: the usage ratio of the intermediate 5, propylene carbonate and chloroform in step s6 is 10 mmol:42-45 mmol:120-150 mL.

[0038] As a further solution of the present invention: the usage ratio of the intermediate 6, diphenylmethane diisocyanate, dibutyltin dilaurate and N,N-dimethylformamide in step s7 is 10 mmol: 20 mmol: 0.01-0.03 g: 120-150 mL.

[0039] As a further solution of the present invention: the water-resistant and anti-fouling water-based environmentally friendly ink is prepared according to the preparation method of the water-resistant and anti-fouling water-based environmentally friendly ink.

[0040] Beneficial effects of the present invention:

[0041] The invention discloses a water-resistant and antifouling water-based environmentally friendly ink and a preparation method thereof. The water-resistant and antifouling resin, ethanol and deionized water are added into a mixer and stirred and mixed, and then pigment, polyethylene wax, titanium dioxide and DC-65 defoamer are added and stirred and mixed to obtain the water-resistant and antifouling water-based environmentally friendly ink. In the process of preparing the water-based environmentally friendly ink, the preparation method first prepares a water-resistant and antifouling resin, firstly performs a chloromethylation reaction on biphenyl to introduce a chlorine atom to obtain an intermediate 1, then the chlorine atom on the intermediate 1 reacts with a hydroxyl group on 3,5-dimethoxyphenol to obtain an intermediate 2, then the methoxy group on the intermediate 2 is converted into a hydroxyl group to obtain an intermediate 3, then the hydroxyl group on the intermediate 3 reacts with a chlorine atom on 2-chloro-5-nitrotrifluorotoluene to obtain an intermediate 4, and then the nitro group on the intermediate 4 is reacted with water. Hydrazine is reduced to amino group to obtain intermediate 5, then the amino group on intermediate 5 reacts with propylene carbonate to introduce carbon chain and hydroxyl group to obtain intermediate 6, then the hydroxyl group on intermediate 6 is polymerized with isocyanate group on diphenylmethane diisocyanate to form water-resistant and antifouling resin; the molecular structure of the water-resistant and antifouling resin contains carbon chain to give it good flexibility, and contains a large number of benzene rings to give it good rigidity and stability, so that it is not easy to be destroyed, and it also contains a large number of CF bonds, the CF bonds have large bond energy and good stability, are not easy to be destroyed, and can reduce its surface energy, show good hydrophobicity, thereby improving its water resistance, and can also show excellent waterproof and oil-proof effect, avoid stains, and achieve anti-fouling effect. Therefore, the environmentally friendly ink using the water-resistant and antifouling resin as the main raw material has good water resistance and stain resistance. DETAILED DESCRIPTION

[0042] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] Embodiment 1:

[0044] This embodiment is a method for preparing a water-resistant and antifouling resin, comprising the following steps:

[0045] Step s1: 0.1 mol biphenyl, 7 g paraformaldehyde, 8 mL of 36% concentrated hydrochloric acid, 25 mL of glacial acetic acid, 0.2 mol zinc chloride and 80 mL cyclohexane are added to a three-necked flask equipped with a thermometer, a stirrer and an air duct, and stirred for reaction at 35°C and a stirring rate of 400 r / min for 30 min, then heated to 45°C and introduced with stirring hydrogen chloride gas until the reaction system is saturated, and then stirred at a constant temperature for 6 h. After the reaction is completed, the reaction product is cooled to room temperature, then added to distilled water, then allowed to stand for stratification, the water layer is removed, and then washed with distilled water until neutral, then cooled to below 0°C, a precipitate is precipitated, and then vacuum filtered, the filter cake is placed in a vacuum drying oven, and dried at 90°C for 2 h to obtain intermediate 1;

[0046] Step s2: 0.1 mol intermediate 1, 0.2 mol 3,5-dimethoxyphenol, 0.22 mol anhydrous potassium carbonate, 120 mL N, N-dimethylacetamide and 50 mL toluene are added to a three-necked flask equipped with a stirrer, a thermometer, a gas duct and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred at 25° C. and a stirring rate of 400 r / min for 20 minutes, and then the mixture is heated to 140° C. and stirred for 10 hours. After the reaction is completed, the reaction product is cooled to room temperature, and then added to distilled water to precipitate, and vacuum filtered. The filter cake is washed with distilled water for 3 times, and then recrystallized with a mixed solvent of equal volumes of anhydrous ethanol and acetone to obtain intermediate 2;

[0047] Step s3: 10 mmol of intermediate 2 and 20 mL of dichloromethane were added to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, and 80 mL of a 1 mol / L boron tribromide solution formed by dissolving boron tribromide in dichloromethane was added dropwise while stirring at a temperature of -10°C and a stirring rate of 400 r / min. The dropping rate was controlled to be 1 drop / s. After the dropwise addition was completed, the stirring reaction was continued for 6 hours. After the reaction was completed, the reaction product was added to a saturated sodium bicarbonate solution, and then vacuum filtered. The filter cake was washed with distilled water 3 times, and then recrystallized with a 70% by volume ethanol solution to obtain intermediate 3;

[0048] Step s4: 10 mmol of intermediate 3, 45 mmol of anhydrous potassium carbonate, 120 mL of N, N-dimethylacetamide and 50 mL of toluene were added to a three-necked flask equipped with a stirrer, a thermometer, a gas duct and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at 140°C and a stirring rate of 400 r / min for 1 hour, and then 40 mmol of 2-chloro-5-nitrotrifluorotoluene was added and the stirring reaction was continued for 10 hours. After the reaction was completed, the reaction product was cooled to room temperature, and then added to distilled water to precipitate, and vacuum filtered. The filter cake was washed with distilled water for 3 times, and then placed in a vacuum drying oven and dried at 80°C for 3 hours to obtain intermediate 4;

[0049] Step s5: 10 mmol of intermediate 4, 0.2 g of 10% palladium carbon and 100 mL of anhydrous ethanol were added to a four-necked flask equipped with a thermometer, a stirrer, an air guide tube, a constant pressure dropping funnel and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred for reaction at 25°C and a stirring rate of 400 r / min for 10 min, and then the temperature was raised to reflux and 15 mL of 50% hydrazine hydrate solution was added dropwise while stirring. The dropping rate was controlled to 1 drop / s. After the addition was completed, the stirring reaction was continued for 8 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered. The filtrate was rotary evaporated to remove the solvent to obtain intermediate 5;

[0050] Step s6: 10 mmol of intermediate 5, 42 mmol of propylene carbonate and 120 mL of chloroform were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at a stirring rate of 400 r / min and heated to reflux for 4 h. The heating rate was controlled to be 2°C / min. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation, and then recrystallized from anhydrous ethanol to obtain intermediate 6;

[0051] Step s7: Add 10 mmol of intermediate 6, 20 mmol of diphenylmethane diisocyanate, 0.01 g of dibutyltin dilaurate and 120 mL of N,N-dimethylformamide into a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir the reaction at 40°C and a stirring rate of 400 r / min for 1 hour, then raise the temperature to 85°C and continue stirring the reaction for 4 hours. After the reaction is completed, the reaction product is cooled to room temperature, then placed in a vacuum drying oven, and dried at 60°C for 8 hours to obtain a water-resistant and antifouling resin.

[0052] Embodiment 2:

[0053] This embodiment is a method for preparing a water-resistant and antifouling resin, comprising the following steps:

[0054] Step s1: 0.1 mol biphenyl, 8 g paraformaldehyde, 10 mL of 38% concentrated hydrochloric acid, 30 mL of glacial acetic acid, 0.25 mol zinc chloride and 100 mL cyclohexane are added to a three-necked flask equipped with a thermometer, a stirrer and an air duct, and stirred for reaction at a temperature of 40°C and a stirring rate of 500 r / min for 40 min, and then heated to 50°C and introduced hydrogen chloride gas while stirring until the reaction system is saturated, and then stirred at a constant temperature for 8 h. After the reaction is completed, the reaction product is cooled to room temperature, and then added to distilled water, and then allowed to stand for stratification, the water layer is removed, and then washed with distilled water until neutral, and then cooled to below 0°C to precipitate, and then vacuum filtered, and the filter cake is placed in a vacuum drying oven and dried at a temperature of 95°C for 3 h to obtain intermediate 1;

[0055] Step s2: 0.1 mol intermediate 1, 0.2 mol 3,5-dimethoxyphenol, 0.25 mol anhydrous potassium carbonate, 150 mL N, N-dimethylacetamide and 60 mL toluene are added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 30° C. and a stirring rate of 500 r / min for 30 min, and then the temperature is raised to 145° C. and the stirring reaction is continued for 15 h. After the reaction is completed, the reaction product is cooled to room temperature, and then added to distilled water to precipitate, and vacuum filtered. The filter cake is washed with distilled water for 5 times, and then recrystallized with a mixed solvent of equal volumes of anhydrous ethanol and acetone to obtain intermediate 2;

[0056] Step s3: 10 mmol of intermediate 2 and 25 mL of dichloromethane were added to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, and a 1.2 mol / L boron tribromide solution of 100 mL of boron tribromide dissolved in dichloromethane was added dropwise while stirring at a temperature of -10°C and a stirring rate of 500 r / min. The dropping rate was controlled to be 2 drops / s. After the dropwise addition was completed, the stirring reaction was continued for 8 hours. After the reaction was completed, the reaction product was added to a saturated sodium bicarbonate solution, and then vacuum filtered. The filter cake was washed with distilled water 5 times, and then recrystallized with an ethanol solution with a volume fraction of 80% to obtain intermediate 3;

[0057] Step s4: 10 mmol of intermediate 3, 50 mmol of anhydrous potassium carbonate, 150 mL of N, N-dimethylacetamide and 60 mL of toluene were added to a three-necked flask equipped with a stirrer, a thermometer, a gas duct and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at 150° C. and a stirring rate of 500 r / min for 2 h, and then 40 mmol of 2-chloro-5-nitrotrifluorotoluene was added and the stirring reaction was continued for 15 h. After the reaction was completed, the reaction product was cooled to room temperature, and then added to distilled water to precipitate, and vacuum filtered. The filter cake was washed with distilled water for 5 times, and then placed in a vacuum drying oven and dried at 85° C. for 5 h to obtain intermediate 4;

[0058] Step s5: 10 mmol of intermediate 4, 0.3 g of 10% palladium carbon and 120 mL of anhydrous ethanol were added to a four-necked flask equipped with a thermometer, a stirrer, an air guide tube, a constant pressure dropping funnel and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred for reaction at 30°C and a stirring rate of 500 r / min for 15 min, and then the temperature was raised to reflux and 20 mL of a 60% hydrazine hydrate solution was added dropwise while stirring. The dropping rate was controlled to 2 drops / s. After the addition was completed, the stirring reaction was continued for 10 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 5;

[0059] Step s6: 10 mmol of intermediate 5, 45 mmol of propylene carbonate and 150 mL of chloroform were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at a stirring rate of 500 r / min and heated to reflux for 5 h. The heating rate was controlled to be 4°C / min. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation, and then recrystallized from anhydrous ethanol to obtain intermediate 6;

[0060] Step s7: Add 10 mmol of intermediate 6, 20 mmol of diphenylmethane diisocyanate, 0.03 g of dibutyltin dilaurate and 150 mL of N,N-dimethylformamide into a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir the reaction at a temperature of 45°C and a stirring rate of 500 r / min for 2 hours, then raise the temperature to 90°C and continue stirring the reaction for 5 hours. After the reaction is completed, the reaction product is cooled to room temperature, then placed in a vacuum drying oven, and dried at a temperature of 65°C for 10 hours to obtain a water-resistant and antifouling resin.

[0061] Embodiment 3:

[0062] This embodiment is a method for preparing a water-resistant and anti-fouling water-based environmentally friendly ink, comprising the following steps:

[0063] Step 1: Weigh 50 parts of the water-resistant and antifouling resin from Example 1, 8 parts of pigment, 2 parts of polyethylene wax, 4 parts of titanium dioxide, 0.8 parts of DC-65 defoamer, 12 parts of ethanol and 20 parts of deionized water according to weight parts for later use; the pigment is benzidine yellow G;

[0064] Step 2: Add the water-resistant and antifouling resin, ethanol and deionized water into a mixer, stir and mix for 1 hour at a stirring rate of 1000 r / min, then add the pigment, polyethylene wax, titanium dioxide and DC-65 defoaming agent and continue stirring and mixing for 2 hours to obtain the water-resistant and antifouling water-based environmentally friendly ink.

[0065] Embodiment 4:

[0066] This embodiment is a method for preparing a water-resistant and anti-fouling water-based environmentally friendly ink, comprising the following steps:

[0067] Step 1: Weigh 70 parts of the water-resistant and antifouling resin from Example 2, 15 parts of pigment, 7 parts of polyethylene wax, 8 parts of titanium dioxide, 1.4 parts of DC-65 defoamer, 20 parts of ethanol and 30 parts of deionized water according to weight parts for later use; the pigment is benzidine yellow G;

[0068] Step 2: Add water-resistant and antifouling resin, ethanol and deionized water into a mixer, stir and mix for 2 hours at a stirring rate of 1500r / min, then add pigment, polyethylene wax, titanium dioxide and DC-65 defoaming agent and continue stirring and mixing for 3 hours to obtain the water-resistant and antifouling water-based environmentally friendly ink.

[0069] Comparative Example 1:

[0070] The difference between Comparative Example 1 and Example 4 is that the environmentally friendly alcohol ester soluble polyurethane ink resin TDD3057L is used instead of the water-resistant and antifouling resin.

[0071] Comparative Example 2:

[0072] Comparative Example 2 is a water-based ink prepared according to the method in Example 1 of the water-based ink and preparation method thereof of application number CN201710959613.1.

[0073] The aqueous inks in Examples 3-4 and Comparative Examples 1-2 were applied onto printing paper, and then the inks were dried. Water was then dripped onto the application location to observe the ink contact angle on the printing paper surface. The water samples were then retained for 2 hours to test the ink water absorption and appearance.

[0074] sample Example 3 Example 4 Comparative Example 1 Comparative Example 2 Contact angle,° 145.8 153.3 112.7 124.8 Water absorption, % 0.35 0.31 1.24 0.52 Appearance No deformation, no blistering No deformation, no blistering Deformed and bubbling No deformation, no blistering

[0075] Referring to the data in the above table, according to the comparison between Examples 3-4 and Comparative Examples 1-2, it can be seen that adding the water-resistant and anti-fouling resin in the present application has better water resistance and stain resistance than adding the environmentally friendly alcohol ester soluble polyurethane ink resin TDD3057L, and the prepared water-based ink has better performance than the water-based ink in the prior art.

[0076] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0077] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a water-resistant and antifouling water-based environmentally friendly ink, characterized in that: The following steps are involved: Step 1: Weigh 50-70 parts of water-resistant and antifouling resin, 8-15 parts of pigment, 2-7 parts of polyethylene wax, 4-8 parts of titanium dioxide, 0.8-1.4 parts of DC-65 defoamer, 12-20 parts of ethanol and 20-30 parts of deionized water according to weight parts, and set aside; Step 2: Add the water-resistant and antifouling resin, ethanol and deionized water into a mixer, stir and mix for 1-2 hours at a stirring rate of 1000-1500 r / min, then add the pigment, polyethylene wax, titanium dioxide and DC-65 defoamer and continue to stir and mix for 2-3 hours to obtain the water-resistant and antifouling water-based environmentally friendly ink; The water-resistant and antifouling resin is prepared by the following steps: Step s1: adding biphenyl, paraformaldehyde, concentrated hydrochloric acid, glacial acetic acid, zinc chloride and cyclohexane into a three-necked flask and stirring for reaction, then introducing hydrogen chloride gas while stirring and reacting at a constant temperature, cooling the reaction product after the reaction is completed, then adding it into distilled water, then standing for stratification, removing the water layer, then washing with distilled water, then cooling to precipitate, then vacuum filtering, and drying the filter cake to obtain intermediate 1; Step s2: adding intermediate 1, 3,5-dimethoxyphenol, anhydrous potassium carbonate, N,N-dimethylacetamide and toluene into a three-necked flask and stirring for reaction. After the reaction is completed, the reaction product is cooled and then added into distilled water to precipitate, vacuum filtered, the filter cake is washed, and then recrystallized to obtain intermediate 2; Step s3: Add intermediate 2 and dichloromethane to a three-necked flask, add boron tribromide solution dropwise while stirring, continue stirring to react after the addition is complete, add the reaction product to a saturated sodium bicarbonate solution after the reaction is complete, then vacuum filter, wash the filter cake, and then recrystallize to obtain intermediate 3; Step s4: adding intermediate 3, anhydrous potassium carbonate, N,N-dimethylacetamide and toluene into a three-necked flask and stirring for reaction, then adding 2-chloro-5-nitrotrifluorotoluene and continuing stirring for reaction, cooling the reaction product after the reaction is completed, then adding it into distilled water to precipitate, vacuum filtering, washing the filter cake and drying it to obtain intermediate 4; Step s5: Add intermediate 4, 10% palladium carbon and anhydrous ethanol to a four-necked flask and stir to react, then heat and add hydrazine hydrate solution dropwise while stirring, continue stirring to react after the addition is complete, cool the reaction product after the reaction is complete, then vacuum filter, and rotary evaporate the filtrate to obtain intermediate 5; Step s6: adding intermediate 5, propylene carbonate and chloroform into a three-necked flask and stirring for reaction. After the reaction is completed, the reaction product is cooled, then rotary evaporated, and then recrystallized to obtain intermediate 6; Step s7: Add intermediate 6, diphenylmethane diisocyanate, dibutyltin dilaurate and N,N-dimethylformamide into a three-necked flask and stir to react. After the reaction is completed, cool the reaction product and then dry it to obtain a water-resistant and antifouling resin.

2. The method for preparing a water-resistant and antifouling water-based environmentally friendly ink according to claim 1, characterized in that: The pigment in step 1 is one of benzidine yellow G, litho scarlet, phthalocyanine blue, phthalocyanine green, phthalocyanine violet and carbon black, or a mixture of two or more thereof in any proportion.

3. The method for preparing a water-resistant and antifouling water-based environmentally friendly ink according to claim 1, characterized in that: The usage ratio of the biphenyl, paraformaldehyde, concentrated hydrochloric acid, glacial acetic acid, zinc chloride and cyclohexane in step s1 is 0.1 mol: 7-8 g: 8-10 mL: 25-30 mL: 0.2-0.25 mol: 80-100 mL, and the mass fraction of the concentrated hydrochloric acid is 36-38%.

4. The method for preparing a water-resistant and antifouling water-based environmentally friendly ink according to claim 1, characterized in that: The usage ratio of the intermediate 1, 3,5-dimethoxyphenol, anhydrous potassium carbonate, N,N-dimethylacetamide and toluene in step s2 is 0.1 mol: 0.2 mol: 0.22-0.25 mol: 120-150 mL: 50-60 mL.

5. The method for preparing a water-resistant and antifouling water-based environmentally friendly ink according to claim 1, characterized in that: The usage ratio of the intermediate 2, dichloromethane and boron tribromide solution in step s3 is 10 mmol: 20-25 mL: 80-100 mL, and the boron tribromide solution is a 1-1.2 mol / L solution formed by dissolving boron tribromide in dichloromethane.

6. The method for preparing a water-resistant and antifouling water-based environmentally friendly ink according to claim 1, characterized in that: The usage ratio of the intermediate 3, anhydrous potassium carbonate, N,N-dimethylacetamide, toluene and 2-chloro-5-nitrotrifluorotoluene in step s4 is 10 mmol: 45-50 mmol: 120-150 mL: 50-60 mL: 40 mmol.

7. The method for preparing a water-resistant and antifouling water-based environmentally friendly ink according to claim 1, characterized in that: The usage ratio of the intermediate 4, 10% palladium carbon, anhydrous ethanol and hydrazine hydrate solution in step s5 is 10 mmol: 0.2-0.3 g: 100-120 mL: 15-20 mL, and the mass fraction of the hydrazine hydrate solution is 50-60%.

8. The method for preparing a water-resistant and antifouling water-based environmentally friendly ink according to claim 1, characterized in that: The usage ratio of the intermediate 5, propylene carbonate and chloroform in step s6 is 10 mmol:42-45 mmol:120-150 mL.

9. The method for preparing a water-resistant and antifouling water-based environmentally friendly ink according to claim 1, characterized in that: The usage ratio of the intermediate 6, diphenylmethane diisocyanate, dibutyltin dilaurate and N,N-dimethylformamide in step s7 is 10mmol:20mmol:0.01-0.03g:120-150mL.

10. A water-resistant and anti-fouling water-based environmentally friendly ink, characterized in that: The water-resistant and anti-fouling water-based environmentally friendly ink is prepared according to the preparation method of the water-resistant and anti-fouling water-based environmentally friendly ink according to any one of claims 1-9.

Citation Information

Patent Citations

  • Water-based ink and preparation method thereof

    CN107556814A

  • Antifouling water-resistant magic tape and manufacture method thereof

    CN102864644A

  • Multi-cyandiamine monomer and preparation and application thereof

    CN103193674A