A method for preparing LTA molecular sieve nanocrystal mixed matrix membrane

By using hydrothermal treatment of silicon source, aluminum source and alkali source and ultrasonic magnetic stirring technology during the synthesis process of LTA molecular sieve nanocrystals, a highly dispersible LTA molecular sieve nanocrystal mixed matrix film was prepared, which solved the problems of inorganic/organic interface defects and agglomeration. , improves the separation performance and pressure resistance of the membrane, and is suitable for CO2 separation and purification.

CN117732255BActive Publication Date: 2024-10-11DALIAN UNIV OF TECH PANJIN INST OF IND TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311781239.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-21
Publication Date
2024-10-11
Estimated Expiration
2043-12-21

AI Technical Summary

Technical Problem

In the existing technology, the synthesis process of LTA molecular sieve nanocrystals is complex and inefficient, and inorganic/organic interface defects and inorganic particle agglomeration affect the gas diffusion path, resulting in reduced membrane separation performance.

Method used

The silicon source, aluminum source and alkali source are mixed with water, dried, ground and aged and crystallized with the assistance of steam to obtain LTA molecular sieve nanocrystals, which are then dispersed in the polymer matrix solution and processed through ultrasonic and magnetic forces. The casting liquid is prepared by stirring, and is defoamed to form a film to form an LTA molecular sieve nanocrystal mixed matrix film.

Benefits of technology

LTA molecular sieve nanocrystals with high dispersion and low agglomeration have been achieved, which improves the gas permeability and separation purity of the membrane, enhances the pressure resistance and anti-pollution performance, and is suitable for CO2 separation and purification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117732255B_ABST
    Figure CN117732255B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing an LTA molecular sieve nanocrystal mixed matrix membrane, the steps of which include: mixing a silicon source, an aluminum source, an alkali source and water and then drying to obtain a solid mixture; grinding the solid mixture and then aging and crystallizing it under the assistance of steam to obtain a crystalline product; washing, drying and calcining the crystalline product to obtain an LTA type molecular sieve nanocrystal; dispersing the LTA type molecular sieve nanocrystal in a polymer matrix solution to obtain a casting solution; degassing the casting solution and forming a film to obtain an LTA molecular sieve nanocrystal mixed matrix membrane. The present invention provides a method for preparing an LTA molecular sieve nanocrystal mixed matrix membrane, which can effectively reduce the problems of interface defects and inorganic particle agglomeration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of LTA molecular sieve membrane preparation, and in particular to a method for preparing an LTA molecular sieve nanocrystal mixed matrix membrane. Background Art

[0002] Traditional separation technologies generally include absorption, adsorption, low-temperature distillation, etc. These methods have disadvantages such as cumbersome operation, high cost, large volume, and high energy consumption. In contrast, membrane separation technology is regarded as an effective means of solving global problems in the environment and energy in separation technology. Membrane separation technology has significant advantages such as high selectivity, easy modular design, simple operation, low energy consumption, and low cost. It is widely used in energy, electricity, petroleum, chemical and other industries, especially in the field of CO2 separation. Compared with traditional CO2 separation technology, membrane separation technology has unique advantages.

[0003] Mixed matrix membranes (MMMs) are a general term for membranes made by uniformly distributing filler particles in a polymer matrix. It combines the advantages of polymer processability, strong mechanical properties and low cost, as well as the advantages of fillers in gas permeability and selectivity, and is expected to break through the trade-off effect between the permeability and selectivity of polymer membranes. At the same time, the preparation of mixed matrix membranes can utilize the existing mature processes for preparing polymer membranes, avoiding the difficulties faced in the preparation of crystalline material membranes, such as high difficulty, high cost, and difficulty in scale-up. Therefore, mixed matrix membranes have attracted the attention and research of many researchers in the field of membrane separation.

[0004] The addition of inorganic fillers, especially porous fillers, effectively increases the free volume fraction of the polymer, reduces the entanglement between polymer molecular segments, and reduces the mass transfer resistance of gas molecules in the membrane, thereby greatly improving the gas permeability of the mixed matrix membrane. However, due to the presence of the interfacial phase, the gas will choose the one with smaller diffusion resistance between the filler pores and the interfacial phase channel for penetration, so the state of the interfacial phase directly affects the working efficiency of the filler. When the interfacial phase is small, the gas will diffuse in the continuous filler pores, but due to the limited pore openings of the porous material, the gas transmission path may be extended. When the interfacial phase is relatively obvious, the interface defects may be connected to a pinhole-like structure due to the aggregation of the filler, giving the gas the opportunity to penetrate directly through the connected interface, resulting in the complete loss of selectivity of the mixed matrix membrane.

[0005] In order to improve the gas separation performance of mixed matrix membranes, the filler should provide a low-resistance pore structure with high gas permeability and sieving properties within the matrix, and interact strongly with the polymer matrix to reduce the size of the interfacial phase. However, inorganic / organic interface defects and agglomeration of inorganic particles will affect the gas diffusion path, resulting in reduced membrane separation performance.

[0006] Molecular sieves are inorganic materials with high dispersibility and low agglomeration, especially LTA molecular sieves, which often have the characteristics of large external specific surface area, small particle size, multiple pore openings, better performance of pore characteristics, and improved membrane separation performance. Therefore, LTA molecular sieves are widely used in catalysis, separation, ion exchange and other fields. However, the currently produced LTA molecular sieves are mostly porous materials with a particle size of more than 1μm, which limits the effective performance of their pore characteristics, especially their application in the fields of catalysis and adsorption. Therefore, in order to improve the adsorption and catalytic performance, LTA molecular sieves need to have the following properties: (1) Have a larger external specific surface area to increase the number of active centers; (2) The reduction of particle size is conducive to the diffusion of reactants and products, thereby improving the catalyst efficiency and making ion exchange easier to occur; (3) Have more pore openings to reduce the possibility of reactants blocking the pores, extend the catalyst operation cycle, and make ion exchange more fully carried out in the pores.

[0007] In addition, the current methods for synthesizing LTA molecular sieve nanocrystals often have technical defects to varying degrees, such as complex process, low synthesis efficiency, difficulty in separating and collecting nano molecular sieves from mother liquor, the need for a large amount of structure-directing agents and mineralizers, high synthesis cost, and the discharge of a large amount of waste liquid that pollutes the environment. This greatly limits the industrial production and application of LTA molecular sieve nanocrystals.

[0008] Therefore, it is of great significance and value to develop a green and simple synthesis route for LTA molecular sieve nanocrystals and use them to synthesize mixed matrix membranes to solve the problems of inorganic / organic interface defects and agglomeration of inorganic particles. Summary of the invention

[0009] The purpose of the present invention is to provide a method for preparing a mixed matrix membrane of LTA molecular sieve nanocrystals in order to address the problems of inorganic / organic interface defects and agglomeration of inorganic particles in the prior art, which affect the gas diffusion path and lead to reduced membrane separation performance, as well as the complex synthesis process and low synthesis efficiency of LTA molecular sieve nanocrystals. The molecular sieve prepared by this method has the characteristics of high dispersibility and low agglomeration, and can better exert the pore characteristics of the molecular sieve. This molecular sieve has advantages in terms of external specific surface area, particle size and number of pore openings, and the mixed matrix membrane prepared using it as a filler can effectively reduce the problems of interface defects and agglomeration of inorganic particles.

[0010] In order to solve the above technical problems, the present invention provides a method for preparing a LTA molecular sieve nanocrystal mixed matrix membrane, comprising the following steps:

[0011] Mixing a silicon source, an aluminum source, an alkali source and water and drying the mixture to obtain a solid mixture;

[0012] The solid mixture is ground and then aged and crystallized with the assistance of steam to obtain a crystalline product;

[0013] The crystallized product is washed, dried and calcined to obtain LTA type molecular sieve nanocrystals;

[0014] Dispersing LTA type molecular sieve nanocrystals in a polymer matrix solution to obtain a casting solution;

[0015] The casting solution is degassed and then formed into a film to obtain an LTA molecular sieve nanocrystal mixed matrix membrane.

[0016] Furthermore, the silicon source, aluminum source, alkali source and water are uniformly mixed in a molar ratio of 1:(0.1-1):(0.1-2):(20-800) and then dried at a temperature of 20-80°C.

[0017] Further, the silicon source is one or more of white carbon black, porous silicon and silica sol;

[0018] The aluminum source is one or more of aluminum isopropoxide, sodium metaaluminate, aluminum hydroxide, aluminum chloride and aluminum sulfate;

[0019] The alkali source is one or more of sodium hydroxide, potassium hydroxide, calcium hydroxide, magnesium hydroxide, ammonia water and ethylenediamine.

[0020] Furthermore, the step of aging and crystallizing the solid mixture with the assistance of steam after grinding comprises:

[0021] Grind the solid mixture and transfer it into an open glass container, place the glass container in the liner of a hydrothermal reactor, and add 5 to 25 mL of deionized water into the liner;

[0022] Aging the mixture at a temperature of 20 to 70° C. for 1 to 12 days;

[0023] The mixture is crystallized at a temperature of 20 to 120° C. and a crystallization time of 1 to 8 days.

[0024] Furthermore, the calcination treatment of the crystal product is carried out in an air atmosphere, the calcination temperature is 240 to 550° C., and the calcination time is 3 to 12 hours.

[0025] Furthermore, the polymer matrix solution is prepared by the following method:

[0026] Mix anhydrous ethanol and deionized water in a volume ratio of (5-12):(1-6), and heat to 60-120° C. in an oil bath to obtain a mixed solution;

[0027] The polymer matrix is ​​added to the mixed solution at a solid-liquid mass ratio of (1-10):(90-150), and the mixture is stirred at 60-120° C. for 4-5 hours to obtain a polymer matrix solution.

[0028] Furthermore, the polymer matrix is ​​polyamide copolyether and / or polyimide.

[0029] Furthermore, the step of dispersing the LTA type molecular sieve nanocrystals in the polymer matrix solution to obtain a casting solution includes using ultrasound and magnetic stirring to disperse the LTA type molecular sieve nanocrystals in the polymer matrix solution, the ultrasound time is 15 to 45 minutes, the magnetic stirring speed is 500 to 1000 rpm / min, and the stirring time is 30 to 60 minutes.

[0030] Furthermore, the mass fraction of LTA type molecular sieve nanocrystals in the casting solution is 1 to 40 wt %.

[0031] Furthermore, the step of forming a film to obtain a LTA molecular sieve nanocrystal mixed matrix membrane after degassing the casting solution comprises:

[0032] The casting solution is subjected to ultrasonic degassing for 30 to 240 minutes, and then allowed to stand for 5 to 15 minutes;

[0033] Pour the casting solution onto a polytetrafluoroethylene plate and place it in a constant temperature oven at 40 to 80°C to dry for 12 to 24 hours;

[0034] The mixture is then placed in a vacuum oven and vacuumed for 12 to 24 hours to obtain a LTA molecular sieve nanocrystal mixed matrix membrane.

[0035] The present invention provides a method for preparing a LTA molecular sieve nanocrystal mixed matrix membrane. In the process of synthesizing LTA molecular sieve nanocrystals, no organic template agent needs to be introduced, and the synthesized sample is easy to collect, with high yield, good dispersibility, and uniform sample size. The present invention uses the prepared LTA molecular sieve nanocrystals as fillers to disperse in a polymer matrix solution to prepare an LTA molecular sieve nanocrystal mixed matrix membrane. Due to the efficient screening effect of the LTA molecular sieve nanocrystals, the mixed matrix membrane can achieve separation of target substances at the molecular level, has high separation purity, and high separation efficiency. In addition, the nanocrystalline LTA molecular sieve nanocrystals are tightly combined with the polymer matrix, so that the prepared mixed matrix membrane has a high porosity and air permeability, thereby ensuring the flux stability of the mixed matrix membrane. The uniform mixing of the LTA molecular sieve nanocrystals and the polymer matrix can improve the pressure resistance of the mixed matrix membrane, so that the mixed matrix membrane can still maintain a good separation effect under high pressure conditions and has good pressure resistance. Moreover, the LTA molecular sieve nanocrystal mixed matrix membrane prepared by the present invention has a higher porosity, is conducive to resisting the invasion of pollutants, has a stronger anti-pollution performance, and can increase the service life of the mixed matrix membrane.

[0036] At the same time, the LTA molecular sieve nanocrystal mixed matrix membrane prepared by the present invention can be applied to multiple fields such as petroleum, chemical industry, environmental protection, etc., and has broad market prospects. For example, the LTA molecular sieve nanocrystal mixed matrix membrane prepared by the present invention is used to separate and purify CO2, wherein the CO2 permeation evaluation of the LTA molecular sieve nanocrystal mixed matrix membrane can greatly improve the selectivity of CO2 / N2. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 A flow chart of a method for preparing a LTA molecular sieve nanocrystal mixed matrix membrane provided in an embodiment of the present invention;

[0038] Figure 2 XRD diagram of LTA molecular sieve nanocrystals prepared by the method for preparing LTA molecular sieve nanocrystal mixed matrix membrane provided in an embodiment of the present invention;

[0039] Figure 3 This is a scanning electron microscope image of the LTA molecular sieve nanocrystal mixed matrix membrane prepared by the preparation method of the LTA molecular sieve nanocrystal mixed matrix membrane provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0040] See also Figure 1 The present invention provides a method for preparing a LTA molecular sieve nanocrystal mixed matrix membrane, comprising the following steps:

[0041] Step 1) Mix a silicon source, an aluminum source, an alkali source and water and dry them to obtain a solid mixture.

[0042] The molar ratio of the silicon source, aluminum source, alkali source and water when mixed is 1:(0.1-1):(0.1-2):(20-800). The silicon source, aluminum source, alkali source and water are uniformly mixed and then dried at a temperature of 20-80° C. to obtain a solid mixture.

[0043] The silicon source is one or more of white carbon black, porous silicon and silica sol.

[0044] The aluminum source is one or more of aluminum isopropoxide, sodium metaaluminate, aluminum hydroxide, aluminum chloride and aluminum sulfate.

[0045] The alkali source is one or more of sodium hydroxide, potassium hydroxide, calcium hydroxide, magnesium hydroxide, ammonia water and ethylenediamine.

[0046] Step 2) Grind the obtained solid mixture into powder, then put the powder into an open glass container, and then put the glass container into a reactor, and perform aging and crystallization treatment on the powder in sequence under steam-assisted conditions to obtain a crystalline product.

[0047] Specifically, the solid mixture powder obtained by grinding is loaded into an open glass container, and then the glass container is placed in a hydrothermal reactor liner, 5 to 25 mL of deionized water is added to the reactor liner, and in order to prevent the deionized water added to the hydrothermal reactor liner from boiling and entering the glass container; the liquid level of the added deionized water is sufficiently lower than the height of the bottle mouth of the glass container.

[0048] The hydrothermal reactor is heated, and the deionized water on the lining of the hydrothermal reactor gradually turns into water vapor during the heating process, so that the solid mixture is aged under the condition of water vapor assistance. The aging temperature is 20 to 70° C. and the aging time is 1 to 12 days.

[0049] After the aging is completed, the solid mixture in the glass container is crystallized under the condition of water vapor assistance, wherein the crystallization temperature is 20 to 120° C. and the crystallization time is 1 to 8 days.

[0050] Such a solid mixture, that is, a dry gel system, is subjected to aging and crystallization treatments by introducing a water source through water vapor under steam-assisted conditions, thereby synthesizing a nanocrystalline crystal product.

[0051] Step 3) The crystalline product is washed, dried and calcined in sequence to obtain LTA type molecular sieve nanocrystals.

[0052] The calcination treatment of the washed and dried crystal product is carried out in an air atmosphere, the calcination temperature is controlled at 240-550° C., and the calcination time is 3-12 hours to obtain highly dispersed LTA molecular sieve nanocrystals.

[0053] Step 4) dispersing the prepared LTA type molecular sieve nanocrystals in a polymer matrix solution to obtain a casting solution.

[0054] Specifically, the prepared LTA type molecular sieve nanocrystals are added to a polymer matrix solution, and the LTA type molecular sieve nanocrystals are dispersed in the polymer matrix solution by ultrasonic and magnetic stirring, wherein the ultrasonic time is controlled at 15 to 45 minutes, the magnetic stirring speed is controlled at 500 to 1000 rpm / min, and the stirring time is 30 to 60 minutes to obtain a casting solution.

[0055] The mass fraction of LTA type molecular sieve nanocrystals in the obtained casting solution is 1-40wt%.

[0056] Wherein, the polymer matrix solution is prepared by the following method:

[0057] First, anhydrous ethanol and deionized water are mixed in a volume ratio of (5-12):(1-6), and stirred and heated to 60-120° C. in an oil bath to obtain a mixed solution.

[0058] Then, a polymer matrix is ​​added to the mixed solution at a solid-liquid mass ratio of (1-10):(90-150), and the mixture is stirred at 60-120° C. for 4-5 hours to completely dissolve the polymer matrix to obtain a polymer matrix solution.

[0059] Wherein, the polymer matrix is ​​polyamide copolyether, or polyimide, or a mixture of polyamide copolyether and polyimide.

[0060] Step 5) Degassing the casting solution to form a film to obtain an LTA molecular sieve nanocrystal mixed matrix membrane.

[0061] The prepared casting solution is first subjected to ultrasonic degassing treatment for 30 to 240 minutes, and then allowed to stand for 5 to 15 minutes.

[0062] Then pour the casting liquid onto a clean polytetrafluoroethylene plate, and then put it into a constant temperature oven at 40 to 80°C to dry for 12 to 24 hours.

[0063] Finally, it is placed in a vacuum oven to evacuate and continue to remove the solvent for 12 to 24 hours to obtain an LTA molecular sieve nanocrystal mixed matrix membrane.

[0064] The present invention provides a method for preparing an LTA molecular sieve nanocrystal mixed matrix membrane. The prepared LTA molecular sieve nanocrystal mixed matrix membrane has the characteristics of high dispersibility and low agglomeration, and can better exert the pore characteristics of the molecular sieve. Since the LTA molecular sieve nanocrystals therein have better advantages in terms of external specific surface area, particle size and number of pore openings, the mixed matrix membrane prepared by using it as a filler can effectively reduce the problems of interface defects and inorganic particle agglomeration.

[0065] The following is a detailed description of the method for preparing a LTA molecular sieve nanocrystal mixed matrix membrane provided by the present invention through examples.

[0066] Example 1

[0067] Step 1: Dissolve 0.11 g of sodium hydroxide in 35 mL of water, add 1.2 g of sodium aluminate and stir magnetically for 30 min, then add 1.2 g of white carbon black to obtain a mixture, and dry it at 80°C.

[0068] Step 2: Grind the dried mixture into powder and transfer it into an open glass container. Then transfer the glass container into a hydrothermal reactor liner. Add 10 ml of deionized water to the liner and prevent water outside the glass container from entering the glass container. Aged the mixture at 25° C. under steam-assisted conditions for 3 days. Heat the hydrothermal reactor to 80° C. and crystallize the mixture under steam-assisted conditions for 8 hours to obtain a crystalline product.

[0069] Step 3: Wash the crystal product by centrifugation for 3 times, dry it at 50° C. for 8 hours, and calcine it at 400° C. for 4 hours in a muffle furnace to obtain LTA type molecular sieve nanocrystals.

[0070] See also Figure 2 The LTA type molecular sieve nanocrystals prepared in the embodiment of the present invention are well crystallized, have no amorphous phase, and the peak position can correspond to the standard LTA zeolite spectrum. There are no impurity peaks other than LTA and no other zeolite impurity phases. And because the product particle size is small, the XRD spectrum has a broadening phenomenon, indicating that it is LTA type zeolite nanocrystals.

[0071] Step 4: Weigh 18 mL of ethanol and 9 mL of distilled water, mix them, heat them to 80°C under stirring, then add 1.1 g of Pebax-1657 and keep stirring at 80°C for 5 hours to completely dissolve them to prepare a polymer matrix solution. Disperse 2 g of molecular sieve nanocrystals as fillers evenly into the polymer matrix solution, stir and disperse them by ultrasonication for 30 minutes, and stir and disperse them at a speed of 1000 rpm / min for 60 minutes to obtain a casting solution containing fillers.

[0072] Step 5: ultrasonically degas the casting solution obtained in step 4 for 60 minutes, and let it stand for 10 minutes, then pour it onto a clean polytetrafluoroethylene plate, put it in an 80°C constant temperature oven to dry for 24 hours, and then put it in a vacuum oven to evacuate and continue to remove the solvent for 24 hours to obtain an LTA molecular sieve nanocrystal mixed matrix membrane.

[0073] See also Figure 3 , is a scanning electron microscope image of the LTA molecular sieve nanocrystal mixed matrix membrane prepared in Example 1 of the present invention. Figure 3 It can be seen that the LTA molecular sieve nanocrystal mixed matrix membrane prepared in the embodiment of the present invention is relatively uniform and has good dispersion.

[0074] The LTA molecular sieve nanocrystal mixed matrix membrane prepared in the embodiment of the present invention is used for the separation and purification of CO2. After testing, the separation performance of the LTA molecular sieve nanocrystal mixed matrix membrane prepared in the embodiment of the present invention is PCO2=160.32 Barrer, and the CO2 / N2 selectivity is 82.79. This shows that the use of the LTA molecular sieve nanocrystal mixed matrix membrane prepared in the embodiment of the present invention for the separation and purification of CO2 can greatly improve the CO2 / N2 selectivity.

[0075] Example 2

[0076] Step 1: Dissolve 0.21 g of sodium hydroxide in 40 mL of water, add 1.5 g of sodium aluminate and stir magnetically for 30 min, then add 1.5 g of white carbon black to obtain a mixture, and dry it at 80°C.

[0077] Step 2: Grind the dried mixture into powder and transfer it into an open glass container. Then transfer the glass container into a hydrothermal reactor liner. Add 15 ml of deionized water to the liner and prevent water outside the glass container from entering the glass container. Aged the mixture at 30° C. under steam-assisted conditions for 2 days. Heat the hydrothermal reactor to 80° C. and crystallize the mixture under steam-assisted conditions for 24 hours to obtain a crystalline product.

[0078] Step 3: Wash the crystal product by centrifugation for 3 times, dry it at 50° C. for 8 hours, and calcine it at 400° C. for 4 hours in a muffle furnace to obtain LTA type molecular sieve nanocrystals.

[0079] See also Figure 2 The LTA type molecular sieve nanocrystals prepared in the embodiment of the present invention are well crystallized, have no amorphous phase, and the peak position can correspond to the standard LTA zeolite spectrum. There are no impurity peaks other than LTA and no other zeolite impurity phases. And because the product particle size is small, the XRD spectrum has a broadening phenomenon, indicating that it is LTA type zeolite nanocrystals.

[0080] Step 4: Weigh 18 mL of ethanol and 9 mL of distilled water, mix them, heat them to 80°C under stirring, then add 1.0 g of Pebax-1657 and keep stirring at 80°C for 5 hours to completely dissolve them to prepare a polymer matrix solution. Disperse 1.5 g of molecular sieve nanocrystals as fillers evenly into the polymer matrix solution, stir at a speed of 1000 rpm / min for 30 minutes, and stir and disperse them under ultrasonication for 30 minutes to obtain a casting solution containing fillers.

[0081] Step 5: ultrasonically degas the casting solution obtained in step 4 for 60 minutes, and let it stand for 10 minutes, then pour it onto a clean polytetrafluoroethylene plate, put it in an 80°C constant temperature oven to dry for 24 hours, and then put it in a vacuum oven to evacuate and continue to remove the solvent for 24 hours to obtain an LTA molecular sieve nanocrystal mixed matrix membrane.

[0082] The LTA molecular sieve nanocrystal mixed matrix membrane prepared in the embodiment of the present invention is used for the separation and purification of CO2. After testing, the separation performance of the LTA molecular sieve nanocrystal mixed matrix membrane prepared in the embodiment of the present invention is PCO2=108.00Barrer, and the CO2 / N2 selectivity is 75.79. It can be shown that the use of the LTA molecular sieve nanocrystal mixed matrix membrane prepared in the embodiment of the present invention for the separation and purification of CO2 can greatly improve the CO2 / N2 selectivity.

[0083] Example 3

[0084] Step 1: Dissolve 1.2 g of sodium hydroxide in 40 mL of water, add 0.6 g of aluminum chloride and stir magnetically for 30 min, then add 1.5 g of white carbon black to obtain a mixture, and dry it at 80°C.

[0085] Step 2: Grind the dried mixture into powder and transfer it into an open glass container. Then transfer the glass container into a hydrothermal reactor liner. Add 15 ml of deionized water to the liner and prevent water outside the glass container from entering the glass container. Aged the mixture at 30° C. under steam-assisted conditions for 3 days. Heat the hydrothermal reactor to 80° C. and crystallize the mixture under steam-assisted conditions for 24 hours to obtain a crystalline product.

[0086] Step 3: Wash the crystal product by centrifugation for 3 times, dry it at 60° C. for 8 hours, and calcine it at 500° C. for 4 hours in a muffle furnace to obtain LTA type molecular sieve nanocrystals.

[0087] See also Figure 2 The LTA type molecular sieve nanocrystals prepared in the embodiment of the present invention are well crystallized, have no amorphous phase, and the peak position can correspond to the standard LTA zeolite spectrum. There are no impurity peaks other than LTA and no other zeolite impurity phases. And because the product particle size is small, the XRD spectrum has a broadening phenomenon, indicating that it is LTA type zeolite nanocrystals.

[0088] Step 4: Weigh 18 mL of ethanol and 9 mL of distilled water, mix them, heat them to 80°C under stirring, then add 1.1 g of polyimide and keep stirring at 80°C for 5 hours to completely dissolve them to obtain a polymer matrix solution. Disperse 1.5 g of molecular sieve nanocrystals as fillers evenly into the polymer matrix solution at 1000 rpm / min, stir for 30 minutes, and stir and disperse under ultrasound for 30 minutes to obtain a casting solution containing fillers.

[0089] Step 5: ultrasonically degas the casting solution obtained in step 4 for 60 minutes, and let it stand for 10 minutes, then pour it onto a clean polytetrafluoroethylene plate, put it in an 80°C constant temperature oven to dry for 24 hours, and then put it in a vacuum oven to evacuate and continue to remove the solvent for 24 hours to obtain an LTA molecular sieve nanocrystal mixed matrix membrane.

[0090] The LTA molecular sieve nanocrystal mixed matrix membrane prepared in the embodiment of the present invention is used for the separation and purification of CO2. After testing, the separation performance of the LTA molecular sieve nanocrystal mixed matrix membrane prepared in the embodiment of the present invention is PCO2=110.00Barrer, and the CO2 / N2 selectivity is 69.56. It can be shown that the use of the LTA molecular sieve nanocrystal mixed matrix membrane prepared in the embodiment of the present invention for the separation and purification of CO2 can greatly improve the CO2 / N2 selectivity.

[0091] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a LTA molecular sieve nanocrystal mixed matrix membrane, characterized in that: The steps include: Mixing a silicon source, an aluminum source, an alkali source and water and drying the mixture to obtain a solid mixture; The solid mixture is ground and then aged and crystallized with the assistance of steam to obtain a crystalline product; The crystallized product is washed, dried and calcined to obtain LTA type molecular sieve nanocrystals; Dispersing LTA type molecular sieve nanocrystals in a polymer matrix solution to obtain a casting solution; Degassing the casting solution and forming a film to obtain an LTA molecular sieve nanocrystal mixed matrix membrane; The silicon source, aluminum source, alkali source and water are mixed and then dried at a temperature of 20 to 80°C; The mass fraction of LTA molecular sieve nanocrystals in the casting solution is 1 to 40 wt %; The polymer matrix solution is prepared by the following method: Mix anhydrous ethanol and deionized water in a volume ratio of (5-12):(1-6), and heat to 60-120° C. in an oil bath to obtain a mixed solution; Adding a polymer matrix to the mixed solution at a solid-liquid mass ratio of (1-10):(90-150), stirring at 60-120° C. for 4-5 hours to obtain a polymer matrix solution; The polymer matrix is ​​polyamide copolyether or / and polyimide; The step of forming a film after degassing the casting solution to obtain an LTA molecular sieve nanocrystal mixed matrix membrane comprises: The casting solution is subjected to ultrasonic degassing for 30 to 240 minutes, and then allowed to stand for 5 to 15 minutes; Pour the casting solution onto a polytetrafluoroethylene plate and place it in a constant temperature oven at 40 to 80°C to dry for 12 to 24 hours; The mixture is then placed in a vacuum oven and vacuumed for 12 to 24 hours to obtain a LTA molecular sieve nanocrystal mixed matrix membrane.

2. The method for preparing the LTA molecular sieve nanocrystal mixed matrix membrane according to claim 1, characterized in that: The silicon source, aluminum source, alkali source and water are mixed in a molar ratio of 1:(0.1-1):(0.1-2):(20-800).

3. The method for preparing the LTA molecular sieve nanocrystal mixed matrix membrane according to claim 2, characterized in that: The silicon source is one or more of white carbon black, porous silicon and silica sol; The aluminum source is one or more of aluminum isopropoxide, sodium metaaluminate, aluminum hydroxide, aluminum chloride and aluminum sulfate; The alkali source is one or more of sodium hydroxide, potassium hydroxide, calcium hydroxide, magnesium hydroxide, ammonia water and ethylenediamine.

4. The method for preparing the LTA molecular sieve nanocrystal mixed matrix membrane according to claim 1, characterized in that: The steps of aging and crystallizing the solid mixture after grinding under steam assistance include: Grind the solid mixture and transfer it into an open glass container, place the glass container in the liner of a hydrothermal reactor, and add 5 to 25 mL of deionized water into the liner; Aging the mixture at a temperature of 20 to 70° C. for 1 to 12 days; The mixture is crystallized at a temperature of 20 to 120° C. and a crystallization time of 1 to 8 days.

5. The method for preparing the LTA molecular sieve nanocrystal mixed matrix membrane according to claim 1, characterized in that: The calcination treatment of the crystal product is carried out in an air atmosphere, the calcination temperature is 240 to 550° C., and the calcination time is 3 to 12 hours.

6. The method for preparing the LTA molecular sieve nanocrystal mixed matrix membrane according to claim 1, characterized in that: The step of dispersing the LTA type molecular sieve nanocrystals in the polymer matrix solution to obtain a casting solution comprises using ultrasound and magnetic stirring to disperse the LTA type molecular sieve nanocrystals in the polymer matrix solution, the ultrasound time is 15 to 45 minutes, the magnetic stirring speed is 500 to 1000 rpm / min, and the stirring time is 30 to 60 minutes.