A nano-modified composite grouting material based on mesoporous particle reinforcement and its preparation method and application
By adding mesoporous particles and elastic particle reinforcements to the grouting material, the interface strength and toughness are improved, which solves the problem of insufficient impact work and energy absorption of the inorganic grouting material in the impact tunnel, and achieves higher compression and resistance. The impact performance reduces the sharp deformation of the surrounding rock of the tunnel.
Patent Information
- Application Number
- CN202311837744.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-28
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-12-28
AI Technical Summary
Existing inorganic grouting materials have insufficient impact work and energy absorption when impacting tunnels, leading to problems such as collapse and falling of the roof and floor of the tunnel.
Nano-modified composite grouting materials based on mesoporous particle reinforcement are used. By adding mesoporous structure nanoparticles and elastic particle tougheners, the particle/gelling material interface repulsion is reduced, the interface strength and toughness are improved, and the grouting material is enhanced. Impact resistance.
The compressive strength and impact strength of the grouting material are improved, which can effectively absorb impact work and energy, reduce the sharp deformation of the surrounding rock of the tunnel, and improve the applicability in the tunnel with impact ground pressure.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of grouting material preparation, and in particular, the present invention relates to a nano-modified composite grouting material based on mesoporous particle reinforcement, and a preparation method and application thereof. Background Art
[0002] Rock burst refers to the dynamic phenomenon of sudden and violent destruction of the rock mass around the shaft or working face due to the instantaneous release of elastic deformation, which is manifested as the throwing out of coal blocks and the overall movement of a small amount of coal, accompanied by loud noises, rock vibrations and shock waves, as well as roof and floor collapse, caving and gas outbursts. Grouting modification is an effective solution to achieve rock burst control. The structural design and performance regulation of grouting materials in grouting modification technology are the key core of grouting modification. Inorganic grouting materials represented by ordinary cement have achieved good reinforcement effects in tunnels with simple geological conditions due to their excellent mechanical strength, environmental performance and price advantages. However, in impact tunnels, their impact work and insufficient energy absorption lead to collapse and caving of the tunnel roof and floor. Summary of the invention
[0003] In view of this, the present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, the embodiment of the present invention provides a nano-modified composite grouting material based on mesoporous particle reinforcement and a preparation method and application thereof.
[0004] To achieve the above object, the present invention adopts the following technical solutions:
[0005] In the first aspect, an embodiment of the present invention proposes a nano-modified composite grouting material based on mesoporous particle reinforcement, comprising the following components in parts by weight: 80-100 parts of silicate cement clinker, 5-10 parts of reinforcing agent, 10-15 parts of mesoporous particles, 1-3 parts of elastic particle toughening agent, 0.5-1 parts of interface modifier, 0.1-0.5 parts of interface coupling agent, and 0.1-0.3 parts of dissolution promoter.
[0006] The embodiment of the present invention can reduce the particle / cementitious material interface repulsion, increase the interface area, reduce interface defects, and thereby improve the interface strength and enhance the impact resistance of the grouting material so that it can meet the use requirements of impact tunnels; at the same time, elastic particle toughening agents are introduced to increase the toughness of the grouting material.
[0007] In some embodiments, the enhancer is a mixture of lithium chloride, aluminum sulfate, sodium sulfate, lithium carbonate and sodium silicate, with a mass ratio of 1:1:3:1:5.
[0008] In some embodiments, the mesoporous particles are a mixture of amino hollow mesoporous silica nanoparticles and carboxyl mesoporous silica nanoparticles, and the mass ratio thereof is (3-4):2, preferably 3:2.
[0009] In some embodiments, the elastic particle toughening agent is a mixture of acrylonitrile-butadiene-styrene block copolymer elastomeric particles and styrene-butadiene block copolymer elastic particles, and the mass ratio thereof is (2-4):1, preferably 3:1.
[0010] In some embodiments, the interfacial modifier is perfluorobutylsulfonyl fluoride.
[0011] In some embodiments, the interfacial coupling agent is 3-isocyanatepropyltrimethoxysilane.
[0012] In some embodiments, the solubilizing agent is isopropyl tri(dioctylpyrophosphate) titanate.
[0013] In a second aspect, the embodiment of the present invention further proposes a method for preparing a nano-modified composite grouting material based on mesoporous particle enhancement as described in the first aspect, comprising the following steps:
[0014] S1, weighing silicate cement clinker and reinforcing agent according to their mass fractions, adding appropriate amount of water and stirring and mixing evenly to obtain grouting base material slurry;
[0015] S2, weighing mesoporous particles, elastic particle toughening agent, interface modifier and interface coupling agent according to their mass fractions, adding appropriate amount of water and stirring and mixing to obtain an active mixed solution;
[0016] S3, adding the active mixed solution obtained in step S2 to the grouting base slurry obtained in step S1, and then adding a dissolving agent according to the mass fraction, stirring and mixing, to obtain the mesoporous particle-enhanced nano-modified composite grouting material.
[0017] The preparation method of the mesoporous particle-enhanced nano-modified composite grouting material according to the embodiment of the present invention has simple process, convenient operation, low cost, and is easy to be widely used.
[0018] In some embodiments, in step S1, the stirring and mixing time is 10-15 minutes, preferably 10 minutes; the temperature is 15-30°C, preferably 20°C;
[0019] And / or, in step S2, the stirring and mixing time is 10-15 minutes, preferably 10 minutes; the temperature is 15-30°C, preferably 20°C;
[0020] And / or, in step S3, the stirring and mixing time is 20-30 min, preferably 20 min; the temperature is 15-30°C, preferably 20°C.
[0021] In the third aspect, the embodiment of the present invention also proposes the application of the nano-modified composite grouting material based on mesoporous particle enhancement as described in the first aspect in rock burst tunnel support. When the nano-modified composite grouting material is applied to rock burst tunnel, it can absorb impact work and energy, reduce the rapid deformation of the tunnel surrounding rock, and improve the applicability of the grouting material in rock burst tunnel. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below. Obviously, the described embodiment is a part of the embodiment of the present invention, not all the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the protection scope of the present invention.
[0023] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by those having ordinary skills in the field to which the present invention belongs.
[0024] Where values are described herein as a range, it should be understood that such disclosure includes disclosure of all possible sub-ranges within that range, as well as specific values falling within that range, regardless of whether a specific value or a specific sub-range is explicitly stated.
[0025] Herein, the words "comprises" and "includes" and variations thereof mean that other elements or integers which are permitted but not specifically described may be included.
[0026] In this article, the term "and / or" is merely a term used to describe the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B may represent three situations: A exists alone, A and B exist at the same time, and B exists alone.
[0027] In the first aspect, an embodiment of the present invention provides a nano-modified composite grouting material based on mesoporous particle reinforcement, comprising the following components in parts by weight: 80-100 parts of silicate cement clinker (non-limiting examples: 80 parts, 85 parts, 88 parts, 90 parts, 92 parts, 96 parts, 100 parts), 5-10 parts of reinforcing agent (non-limiting examples: 5 parts, 6 parts, 8 parts, 10 parts), 10-15 parts of mesoporous particles (non-limiting examples: 10 parts, 1 2 parts, 14 parts, 15 parts), elastic particle toughening agent 1-3 parts (non-limiting examples: 1 part, 2 parts, 3 parts), interface modifier 0.5-1 parts (non-limiting examples: 0.5 parts, 0.8 parts, 1 parts), interface coupling agent 0.1-0.5 parts (non-limiting examples: 0.1 parts, 0.2 parts, 0.4 parts, 0.5 parts), dissolution promoter 0.1-0.3 parts (non-limiting examples: 0.1 parts, 0.2 parts, 0.3 parts).
[0028] In some specific embodiments, the enhancer is a mixture of lithium chloride, aluminum sulfate, sodium sulfate, lithium carbonate and sodium silicate, and the mass ratio thereof is 1:1:3:1:5.
[0029] In some specific embodiments, the mesoporous particles are a mixture of amino hollow mesoporous silica nanoparticles and carboxyl mesoporous silica nanoparticles, and the mass ratio is (3-4):2, for example, 3:2, 3.5:2, 3.8:2 or 4:2, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable; further, the mass ratio of the mesoporous particles is preferably 3:2 for the amino hollow mesoporous silica nanoparticles and the carboxyl mesoporous silica nanoparticles. The inventors have found that by adding nanoparticles with mesoporous structures such as amino hollow mesoporous silica nanoparticles and carboxyl mesoporous silica nanoparticles to the grouting material, the interfacial repulsion of the particles / cementitious materials can be reduced, the interfacial area can be increased, the interfacial defects can be reduced, and the interfacial strength can be improved, and the impact resistance of the grouting material can be enhanced, so that it can meet the use requirements of the impact lane.
[0030] In some specific embodiments, the elastic particle toughening agent is a mixture of acrylonitrile-butadiene-styrene block copolymer elastic particles and styrene-butadiene block copolymer elastic particles, and the mass ratio is (2-4):1, for example, it can be 2:1, 2.5:1, 2.8:1, 3:1, 3.3:1, 3.6:1 or 4:1, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable; further, the mass ratio of acrylonitrile-butadiene-styrene block copolymer elastic particles to styrene-butadiene block copolymer elastic particles is preferably 3:1. The inventors have found that by using a mixture of acrylonitrile-butadiene-styrene block copolymer elastic particles and styrene-butadiene block copolymer elastic particles as an elastic particle toughening agent, the toughness of the grouting material can be improved.
[0031] In some specific embodiments, the interfacial modifier is perfluorobutylsulfonyl fluoride.
[0032] In some specific embodiments, the interfacial coupling agent is 3-isocyanatepropyltrimethoxysilane.
[0033] In some specific embodiments, the dissolution promoter is isopropyl tri(dioctyl pyrophosphate) titanate.
[0034] In a second aspect, the embodiment of the present invention further proposes a method for preparing a nano-modified composite grouting material based on mesoporous particle enhancement as described in the first aspect, comprising the following steps:
[0035] S1, weighing silicate cement clinker and reinforcing agent according to their mass fractions, adding appropriate amount of water and stirring and mixing evenly to obtain grouting base material slurry;
[0036] S2, weighing mesoporous particles, elastic particle toughening agent, interface modifier and interface coupling agent according to their mass fractions, adding appropriate amount of water and stirring and mixing to obtain an active mixed solution;
[0037] S3, adding the active mixed solution obtained in step S2 to the grouting base slurry obtained in step S1, and then adding a solvent according to the mass fraction, stirring and mixing, so as to obtain a nano-modified composite grouting material based on mesoporous particle reinforcement.
[0038] The preparation method of the mesoporous particle-enhanced nano-modified composite grouting material according to the embodiment of the present invention has a simple process, is easy to operate, does not require complicated production equipment, and has a low cost.
[0039] In some specific embodiments, in step S1, the stirring and mixing time is 10-15 minutes, for example, it can be 10 minutes, 12 minutes, 14 minutes or 15 minutes, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable, preferably 10 minutes; the temperature is 15-30°C, for example, it can be 15°C, 18°C, 20°C, 25°C, 26°C or 30°C, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable, preferably 20°C;
[0040] And / or, in step S2, the stirring and mixing time is 10-15 min, for example, 10 min, 12 min, 13 min or 15 min, but not limited to the listed values, other values not listed in the numerical range are also applicable, preferably 10 min; the temperature is 15-30°C, for example, 15°C, 18°C, 20°C, 25°C, 26°C or 30°C, but not limited to the listed values, other values not listed in the numerical range are also applicable, preferably 20°C;
[0041] And / or, in step S3, the stirring and mixing time is 20-30 min, for example, it can be 20 min, 25 min, 28 min or 30 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable, preferably 20 min; the temperature is 15-30°C, for example, it can be 15°C, 18°C, 20°C, 25°C, 26°C or 30°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable, preferably 20°C.
[0042] In the third aspect, the embodiment of the present invention also proposes the application of the nano-modified composite grouting material based on mesoporous particle enhancement as described in the first aspect in rock burst tunnel support. When the nano-modified composite grouting material is applied to rock burst tunnel, it can absorb impact work and energy, reduce the rapid deformation of the tunnel surrounding rock, and has a good use effect.
[0043] The technical solution of the present invention is further described in detail below in conjunction with specific examples. Unless otherwise specified, the various raw materials used in the examples are conventional commercial products or can be prepared by known methods.
[0044] Example 1
[0045] This embodiment provides a method for preparing a nano-modified composite grouting material based on mesoporous particle enhancement, comprising the following steps:
[0046] S1, weighing 90 parts of Portland cement clinker and 8 parts of reinforcing agent according to their mass fractions, adding appropriate amount of water and stirring and mixing at 20°C for 10 minutes to obtain a grouting base slurry; wherein the reinforcing agent is a mixture of lithium chloride, aluminum sulfate, sodium sulfate, lithium carbonate and sodium silicate in a mass ratio of 1:1:3:1:5;
[0047] S2, weighing 13 parts of mesoporous particles, 3 parts of elastic particle toughening agent, 0.7 parts of perfluorobutylsulfonyl fluoride and 0.3 parts of 3-isocyanatepropyltrimethoxysilane according to their mass parts, adding appropriate amount of water and stirring and mixing at 20°C for 10 minutes to obtain an active mixed solution; wherein the mesoporous particles are a mixture of amino hollow mesoporous silica nanoparticles and carboxyl mesoporous silica nanoparticles in a mass ratio of 3:2; the elastic particle toughening agent is a mixture of acrylonitrile-butadiene-styrene block copolymer elastomer particles and styrene-butadiene block copolymer elastic particles in a mass ratio of 3:1;
[0048] S3, adding the active mixed solution obtained in step S2 to the grouting base slurry obtained in step S1, and then adding 0.2 parts of isopropyl tri(dioctyl pyrophosphate) titanate according to the mass fraction, stirring and mixing at 20°C for 20 minutes, and obtaining a nano-modified composite grouting material based on mesoporous particle reinforcement.
[0049] Example 2
[0050] This embodiment provides a method for preparing a nano-modified composite grouting material based on mesoporous particle enhancement, comprising the following steps:
[0051] S1, weighing 85 parts of Portland cement clinker and 6 parts of reinforcing agent according to their mass fractions, adding appropriate amount of water and stirring and mixing at 20°C for 10 minutes to obtain a grouting base slurry; wherein the reinforcing agent is a mixture of lithium chloride, aluminum sulfate, sodium sulfate, lithium carbonate and sodium silicate in a mass ratio of 1:1:3:1:5;
[0052] S2, weighing 13 parts of mesoporous particles, 1 part of elastic particle toughening agent, 0.6 parts of perfluorobutylsulfonyl fluoride and 0.2 parts of 3-isocyanatepropyltrimethoxysilane according to their mass parts, adding appropriate amount of water, stirring and mixing at 20°C for 10 minutes to obtain an active mixed solution; wherein the mesoporous particles are a mixture of amino hollow mesoporous silica nanoparticles and carboxyl mesoporous silica nanoparticles in a mass ratio of 3:2; the elastic particle toughening agent is a mixture of acrylonitrile-butadiene-styrene block copolymer elastomer particles and styrene-butadiene block copolymer elastic particles in a mass ratio of 3:1;
[0053] S3, adding the active mixed solution obtained in step S2 to the grouting base slurry obtained in step S1, and then adding 0.2 parts of isopropyl tri(dioctyl pyrophosphate) titanate according to the mass fraction, stirring and mixing at 20°C for 20 minutes, and obtaining a nano-modified composite grouting material based on mesoporous particle reinforcement.
[0054] Example 3
[0055] This embodiment provides a method for preparing a nano-modified composite grouting material based on mesoporous particle enhancement, comprising the following steps:
[0056] S1, weighing 88 parts of Portland cement clinker and 5 parts of reinforcing agent according to their mass fractions, adding appropriate amount of water and stirring and mixing at 20°C for 15 minutes to obtain a grouting base slurry; wherein the reinforcing agent is a mixture of lithium chloride, aluminum sulfate, sodium sulfate, lithium carbonate and sodium silicate in a mass ratio of 1:1:3:1:5;
[0057] S2, weighing 10 parts of mesoporous particles, 3 parts of elastic particle toughening agent, 1 part of perfluorobutylsulfonyl fluoride and 0.4 parts of 3-isocyanatepropyltrimethoxysilane according to their mass parts, adding appropriate amount of water and stirring and mixing at 20°C for 15 minutes to obtain an active mixed solution; wherein the mesoporous particles are a mixture of amino hollow mesoporous silica nanoparticles and carboxyl mesoporous silica nanoparticles in a mass ratio of 3.2:2; the elastic particle toughening agent is a mixture of acrylonitrile-butadiene-styrene block copolymer elastomer particles and styrene-butadiene block copolymer elastic particles in a mass ratio of 3:1;
[0058] S3, adding the active mixed solution obtained in step S2 to the grouting base slurry obtained in step S1, and then adding 0.1 parts of isopropyl tri(dioctyl pyrophosphate) titanate according to the mass fraction, stirring and mixing at 20°C for 20 minutes, and obtaining a nano-modified composite grouting material based on mesoporous particle reinforcement.
[0059] Example 4
[0060] This embodiment provides a method for preparing a nano-modified composite grouting material based on mesoporous particle enhancement, comprising the following steps:
[0061] S1, weighing 80 parts of Portland cement clinker and 6 parts of reinforcing agent according to their mass fractions, adding appropriate amount of water and stirring and mixing at 25°C for 10 minutes to obtain a grouting base slurry; wherein the reinforcing agent is a mixture of lithium chloride, aluminum sulfate, sodium sulfate, lithium carbonate and sodium silicate in a mass ratio of 1:1:3:1:5;
[0062] S2, weighing 12 parts of mesoporous particles, 2 parts of elastic particle toughening agent, 1 part of perfluorobutylsulfonyl fluoride and 0.2 parts of 3-isocyanatepropyltrimethoxysilane according to their mass parts, adding appropriate amount of water and stirring and mixing at 25°C for 10 minutes to obtain an active mixed solution; wherein the mesoporous particles are a mixture of amino hollow mesoporous silica nanoparticles and carboxyl mesoporous silica nanoparticles in a mass ratio of 3:2; the elastic particle toughening agent is a mixture of acrylonitrile-butadiene-styrene block copolymer elastomer particles and styrene-butadiene block copolymer elastic particles in a mass ratio of 3.5:1;
[0063] S3, adding the active mixed solution obtained in step S2 to the grouting base slurry obtained in step S1, and then adding 0.2 parts of isopropyl tri(dioctyl pyrophosphate) titanate according to the mass fraction, stirring and mixing at 20°C for 20 minutes, and obtaining a nano-modified composite grouting material based on mesoporous particle reinforcement.
[0064] Example 5
[0065] This embodiment provides a method for preparing a nano-modified composite grouting material based on mesoporous particle enhancement, comprising the following steps:
[0066] S1, weighing 100 parts of Portland cement clinker and 8 parts of reinforcing agent according to their mass fractions, adding appropriate amount of water and stirring and mixing at 20°C for 10 minutes to obtain a grouting base slurry; wherein the reinforcing agent is a mixture of lithium chloride, aluminum sulfate, sodium sulfate, lithium carbonate and sodium silicate in a mass ratio of 1:1:3:1:5;
[0067] S2, weighing 15 parts of mesoporous particles, 3 parts of elastic particle toughening agent, 0.8 parts of perfluorobutylsulfonyl fluoride and 0.5 parts of 3-isocyanatepropyltrimethoxysilane according to their mass parts, adding appropriate amount of water and stirring and mixing at 20°C for 10 minutes to obtain an active mixed solution; wherein the mesoporous particles are a mixture of amino hollow mesoporous silica nanoparticles and carboxyl mesoporous silica nanoparticles in a mass ratio of 3:2; the elastic particle toughening agent is a mixture of acrylonitrile-butadiene-styrene block copolymer elastomer particles and styrene-butadiene block copolymer elastic particles in a mass ratio of 3:1;
[0068] S3, adding the active mixed solution obtained in step S2 to the grouting base slurry obtained in step S1, and then adding 0.3 parts of isopropyl tri(dioctyl pyrophosphate) titanate according to the mass fraction, stirring and mixing at 20°C for 20 minutes, and obtaining a nano-modified composite grouting material based on mesoporous particle reinforcement.
[0069] The compressive strength and impact strength of the mesoporous particle-reinforced nano-modified composite grouting material prepared in the above embodiment were tested, and the results are shown in Table 1.
[0070] Table 1
[0071] Compressive strength / MPa Impact strength / kJ / m Example 1 51 22 Example 2 47 26 Example 3 49 21 Example 4 47 22 Example 5 53 30
[0072] As can be seen from Table 1, the embodiments of the present invention can reduce the interfacial repulsion of particles / cementitious materials, increase the interfacial area, reduce interfacial defects, and thus improve the interfacial strength, enhance the impact resistance of the grouting material, and enable it to meet the use requirements of impact tunnels by adding nanoparticles with a mesoporous structure such as amino hollow mesoporous silica nanoparticles and carboxyl mesoporous silica nanoparticles to the grouting material; at the same time, by using a mixture of acrylonitrile-butadiene-styrene block copolymer elastomeric particles and styrene-butadiene block copolymer elastic particles as elastic particle toughening agents, the toughness of the grouting material can be improved, and the prepared nano-modified composite grouting material exhibits higher compressive strength and impact strength.
[0073] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0074] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A nano-modified composite grouting material based on mesoporous particle reinforcement, characterized in that: The invention comprises the following components in parts by weight: 80-100 parts of silicate cement clinker, 5-10 parts of reinforcing agent, 10-15 parts of mesoporous particles, 1-3 parts of elastic particle toughening agent, 0.5-1 parts of interface modifier, 0.1-0.5 parts of interface coupling agent, and 0.1-0.3 parts of dissolution promoter; Wherein, the mesoporous particles are a mixture of amino hollow mesoporous silica nanoparticles and carboxyl mesoporous silica nanoparticles, and the mass ratio thereof is (3-4):2; The elastic particle toughening agent is a mixture of acrylonitrile-butadiene-styrene block copolymer elastic particles and styrene-butadiene block copolymer elastic particles, and the mass ratio thereof is (2-4):
1.
2. The mesoporous particle-enhanced nano-modified composite grouting material according to claim 1, characterized in that: The reinforcing agent is a mixture of lithium chloride, aluminum sulfate, sodium sulfate, lithium carbonate and sodium silicate, and the mass ratio thereof is 1:1:3:1:
5.
3. The mesoporous particle-enhanced nano-modified composite grouting material according to claim 1, characterized in that: The interface modifier is perfluorobutylsulfonyl fluoride.
4. The mesoporous particle-enhanced nano-modified composite grouting material according to claim 1, characterized in that: The interface coupling agent is 3-isocyanate propyltrimethoxysilane.
5. The mesoporous particle-enhanced nano-modified composite grouting material according to claim 1, characterized in that: The dissolution promoter is isopropyl tri(dioctyl pyrophosphate) titanate.
6. A method for preparing a mesoporous particle-enhanced nano-modified composite grouting material according to any one of claims 1 to 5, characterized in that: The steps include: S1, weighing silicate cement clinker and reinforcing agent according to their mass fractions, adding appropriate amount of water and stirring and mixing evenly to obtain grouting base material slurry; S2, weighing mesoporous particles, elastic particle toughening agent, interface modifier and interface coupling agent according to their mass fractions, adding appropriate amount of water and stirring and mixing to obtain an active mixed solution; S3, adding the active mixed solution obtained in step S2 to the grouting base slurry obtained in step S1, and then adding a dissolving agent according to the mass fraction, stirring and mixing, to obtain the mesoporous particle-enhanced nano-modified composite grouting material.
7. The method for preparing a mesoporous particle-enhanced nano-modified composite grouting material according to claim 6, characterized in that: In step S1, the stirring and mixing time is 10-15 minutes and the temperature is 15-30°C; And / or, in step S2, the stirring and mixing time is 10-15 minutes and the temperature is 15-30°C; And / or, in step S3, the stirring and mixing time is 20-30 minutes and the temperature is 15-30°C.
8. Use of the mesoporous particle-enhanced nano-modified composite grouting material according to any one of claims 1 to 5 in rock burst tunnel support.