A suspension printing support material supporting cell growth and its preparation method and application
The suspended printing support material combined with bio-based polymers and inorganic nanomaterials solves the problem of constructing large-scale hierarchical vascularized organs in the existing technology, achieves both biocompatibility and mechanical properties, and supports cell growth and suspension in suspension. Freely switch states during printing, suitable for building complex structures.
Patent Information
- Application Number
- CN202311781459.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-12-22
AI Technical Summary
It is difficult to construct large-scale hierarchical vascularized organs with existing technology, mainly because the hierarchical vascular construction materials need to be compatible with cell compatibility and engineering plasticity. Large-scale organ printing takes a long time and cannot support cell survival, and it is difficult to achieve multi-level construction.
The suspension printing support material is a combination of bio-based polymers and inorganic nanomaterials. It has excellent biocompatibility and mechanical properties and can be quickly cured under light or heat trigger conditions. It is suitable for suspension printing to support cell growth and during the printing process. Freely switch between sol and gel states.
A support material that combines biocompatibility and mechanical properties in suspension printing has been achieved to support cell growth and complex structure printing, providing a feasible solution for the construction of large-scale hierarchical vascularized organs.
Smart Images

Figure CN117757276B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of biomaterials, and in particular relates to a suspension printing support material for supporting cell growth, and a preparation method and application thereof. Background Art
[0002] 3D printing technology, as a tissue engineering technology, is based on 3D printing. It uses living cells and bio-based materials as raw materials, accurately controls the positioning of biomaterials, living cells, functional components, etc. in each layer, and prints layer by layer to form a 3D scaffold that can be used for transplantation.
[0003] At present, the main technologies used for biomaterial accumulation and molding are inkjet printing, micro-extrusion printing and light-assisted printing. Among them, the temperature-controlled inkjet printer heats the nozzle to generate pulsed air pressure to print droplets, and the acoustic printer generates pulsed pressure through piezoelectric or ultrasound; the micro-extrusion printer uses a pneumatic or mechanical drive system to extrude continuous small balls or wires containing materials and cells; light-assisted printing uses light to focus on an energy-absorbing substrate to provide a driving force for biomaterial printing; however, it is very difficult to use the above printing methods to print vascularized structures with spatially defined characteristics, and there are currently the following problems in constructing large-scale hierarchical vascularized organs: (1) The construction materials of hierarchical blood vessels need to be compatible with cell compatibility (especially supporting the self-assembly of endothelial cell microvascular networks) and engineering plasticity; (2) The printing time of large-scale organs is long and cannot support cell survival; (3) Large-scale vascularized organs contain tissue structures and vascular structures, and there are at least two different levels of tissue structures, and current printing technology makes it difficult to achieve multi-level construction.
[0004] Suspended 3D printing uses suspended medium materials to provide support, squeezes liquid materials from a syringe into a support bath, and forms a scaffold with a complex 3D structure. The working principle of suspended 3D printing technology requires that the ink material must quickly gel into filaments without spreading. This technology improves the molding stability of 3D bioprinting inks with weaker mechanical strength during the printing process without the need for additional printing support structures. The commonly used suspended medium materials are mainly gelatin microparticles. The size and uniformity of the particles directly affect the printing accuracy, and the preparation process of the support bath is complicated. CN114854042A discloses a suspension medium for suspended 3D bioprinting, and a preparation method and application thereof; the suspension medium provided by the invention includes but is not limited to the following components in mass percentage: 0-10% gellan gum, 0-10% thiolated gellan gum, and solvent remainder; and the contents of gellan gum and thiolated gellan gum are not zero at the same time; the suspension medium provided by the invention has good thixotropy and self-repairing ability, so that the nozzle of the 3D bioprinter can move freely in the suspension medium while maintaining the integrity of the 3D bioprinting structure; it solves the problem that natural polymer materials such as collagen and fibrin in traditional printing cannot achieve self-supporting printing; however, the suspension medium provided by the invention has poor biocompatibility and cannot support cell production.
[0005] Therefore, in response to the above problems, it is urgent to develop a suspension printing support material with excellent mechanical properties and support for cell growth. Summary of the invention
[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a suspension printing support material that supports cell growth, and a preparation method and application thereof. The suspension printing support material is a combination of bio-based polymers and inorganic nanomaterials, which can take into account both printability and biological activity, can preload cells and support cell production, and has excellent mechanical properties. It is suitable for suspension printing and provides a feasible solution for the construction of large-scale hierarchical vascularized organs.
[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a suspension printing support material for supporting cell growth, wherein the suspension printing support material comprises a bio-based polymer and an inorganic nanomaterial.
[0009] The suspension printing support material provided by the present invention is a combination of bio-based polymers and inorganic nanomaterials; wherein the bio-based polymer has excellent biocompatibility and can be rapidly cured under light-induced or heat-induced conditions, while the inorganic nanomaterial has a special structure and charged properties; the inventors of the present invention have found that the composite material formed by combining the above two materials not only has good biocompatibility and can be preloaded with cells, but also has good shear thinning properties and self-supporting properties, and can be freely switched between a sol state (low viscosity) and a gel state (high viscosity) during suspension printing; specifically, during suspension printing, the above composite material is subjected to shear force, and the viscosity is reduced to a sol state, which is convenient for suspension printing. After printing, the shear force disappears, and the composite material can quickly return to a gel state, which is convenient for subsequent curing to form a stable shape and structure;
[0010] In summary, it can be seen that the suspended printing support material provided by the present invention combines the advantages of both bio-based polymers and inorganic nanomaterials, has excellent biocompatibility, mechanical properties and printability, and can be used for suspended printing in cell-laden molds, which increases the complexity of printed organs and provides a feasible solution for the manufacture of hierarchical vascularized large-scale organs.
[0011] Preferably, the mass ratio of the bio-based polymer to the inorganic nanomaterial is 10:(4-12), for example, 10:5, 10:6, 10:7, 10:8, 10:9, 10:10 or 10:11, etc.
[0012] As a preferred technical solution of the present invention, the mass ratio of bio-based polymers and inorganic nanomaterials is further limited to 10: (4-12). If the relative amount of inorganic nanomaterials is low, the mechanical properties of the prepared suspended printing support material will be poor, and the support and printing performance will be poor; if the relative amount of inorganic nanomaterials is high, the biocompatibility of the prepared suspended printing support material will be poor, which is not conducive to cell growth.
[0013] Preferably, the bio-based polymer includes an unmodified bio-based polymer and / or a bio-based polymer modified with a polymer monomer.
[0014] It should be noted that the "bio-based polymer" mentioned in the present invention includes unmodified bio-based polymers and bio-based polymers modified by polymer monomers, and the same expressions mentioned below have the same meanings.
[0015] Preferably, the bio-based polymer in the unmodified bio-based polymer includes any one or a combination of at least two of hyaluronic acid, chondroitin sulfate, heparin sulfate, dextran, alginate, cellulose, chitin, chitosan, gelatin, collagen, silk fibroin, albumin, keratin or elastin.
[0016] Preferably, the polymerizable monomer in the bio-based polymer modified by the polymer monomer comprises any one or a combination of at least two of methacrylate, methacrylamide, acrylate, styrene, hydroxyethyl methacrylate, lactic acid methacrylate, caprolactone methacrylate, norbornene, maleimide, vinyl sulfone, tetrazine, tyramine, catechol, azide-alkyne, imine, hydrazone or disulfide.
[0017] Preferably, the bio-based polymer modified by the polymerizable monomer includes any one of methacryloyl collagen, methacryloyl gelatin, methacryloyl hyaluronic acid, methacryloyl alginate, methacryloyl collagen fibroin, methacryloyl albumin, norbornene collagen, norbornene gelatin, norbornene alginate or norbornene hyaluronic acid, or a combination of at least two thereof.
[0018] Preferably, the inorganic nanomaterial comprises any one of nanoclay, nanohydroxyapatite (nHAP), nanosilicate (nSi), bioactive glass (BGn) or mesoporous silica (MSN), or a combination of at least two thereof.
[0019] Preferably, the suspension printing support material also includes a photoinitiator.
[0020] For the suspension printing support material provided by the present invention, if the bio-based polymer used includes a bio-based polymer modified by a polymer monomer, and can only be subsequently formed by photocuring, then a photoinitiator needs to be added. If the bio-based polymer used is an unmodified bio-based polymer, photocuring or thermal curing can be selected as needed. If thermal curing is selected, then there is no need to add additional photoinitiator.
[0021] Preferably, the photoinitiator is a biocompatible photoinitiator.
[0022] Preferably, the biocompatible photoinitiator comprises a biocompatible ultraviolet photoinitiator or a biocompatible visible light photoinitiator.
[0023] Preferably, the biocompatible UV photoinitiator comprises 2-hydroxy-4-(2-hydroxyethoxy)-2-methylpropiophenone (Irgacure, I2959) and / or ethyl 2,4,6-trimethylbenzoylphenylphosphonate (TPO).
[0024] Preferably, the biocompatible visible light initiator comprises lithium phenyl-2,4,6-trimethylbenzoylphosphinate (LAP).
[0025] In a second aspect, the present invention provides a method for preparing the suspended printing support material as described in the first aspect, the preparation method comprising: reacting a bio-based polymer, an inorganic nanomaterial and optionally a photoinitiator in a solvent to obtain the suspended printing support material.
[0026] Preferably, the solvent comprises sterile water.
[0027] In a third aspect, the present invention provides an artificial vascularized organ, wherein the artificial vascularized organ is obtained by suspension printing using the suspension printing support material and cells as described in the first aspect.
[0028] The artificial vascularized organ provided by the present invention is obtained by suspension printing by combining suspension printing support materials and cells, and thus comprises tissue structures and vascular structures, and at least two levels of different tissue structures exist.
[0029] Preferably, the cells include endothelial cells, fibroblasts, induced pluripotent stem cells, HepG2 cells, A549 cells, 293 cells, Hela cells, MCF7 cells, CHO-K1 cells, mesenchymal stem cells, smooth muscle cells, hematopoietic stem cells, and any one or a combination of at least two of primary cells extracted from the brain, heart, liver, kidney, intestine, stomach, reproductive organs or muscle tissue organs.
[0030] Preferably, the biological ink used in the suspension printing includes any one of gelatin, hydroxyapatite, polylactic acid or polylactic acid-co-lactic acid, or a combination of at least two of them.
[0031] In a fourth aspect, the present invention provides a method for preparing the artificial vascularized organ according to the third aspect, the preparation method comprising the following steps:
[0032] (1) adding cells to the suspension printing support material as described in the first aspect to obtain a suspension bath containing cells;
[0033] (2) Using biological ink to perform suspension printing in the cell-containing suspension bath obtained in step (1), and solidifying to obtain the artificial vascularized organ.
[0034] The preparation method of the artificial vascularized organ provided by the present invention first adds cells to a suspension printing support material. Since the suspension printing support material has excellent biocompatibility and will not affect the activity of the cells, the suspension printing support material carrying the cells is placed in a printing mold as a suspension bath. After solidification, it will serve as a primary printing structure. Bio-ink is then used to perform suspension printing in the above suspension bath, and structures such as spiral spheres, grid structures, and complex letter structures can be manufactured, which can serve as secondary printing structures. Finally, after solidification and removal of the bio-ink, a vascular structure can be formed in the structure.
[0035] Preferably, the curing in step (2) is photocuring or thermal curing.
[0036] Preferably, the intensity of the light curing is 5 to 30 mW / cm 2 , for example 6mW / cm 2 , 7mW / cm 2 , 8mW / cm 2 , 9mW / cm 2 、10mW / cm 2 、11mW / cm 2 , 12mW / cm 2 、13mW / cm 2 、14mW / cm 2 、16mW / cm 2 、18mW / cm 2 , 20mW / cm 2 、22mW / cm 2 , 24mW / cm 2 、26mW / cm 2 or 28mW / cm 2 wait.
[0037] Preferably, the light curing time is 10 to 60 seconds, such as 20 seconds, 30 seconds, 40 seconds or 50 seconds, etc. In a fifth aspect, the present invention provides a use of the artificial vascularized organ as described in the third aspect in organogenesis research, organ pathology research or drug screening research.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] The suspension printing support material for supporting cell growth provided by the present invention comprises a bio-based polymer and an inorganic nanomaterial. The bio-based polymer and the inorganic nanomaterial are used in combination, so that the obtained suspension printing support material can take into account both excellent printability and biological activity, can preload cells and support cell production, and also has excellent mechanical properties and sufficiently strong supporting force, and is suitable for suspension printing. The suspension printing support material is used as a suspension bath to print complex artificial vascularized organs, providing a feasible solution for the printing of hierarchical vascularized large-scale organs. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 A curve diagram showing the change of the storage modulus G' and the loss modulus G" of the suspension printing support material provided in Example 1 with temperature;
[0041] Figure 2 A curve diagram showing the change of storage modulus G' and loss modulus G" of the suspension printing support material provided in Comparative Example 1 with temperature;
[0042] Figure 3 A curve diagram showing the change of the storage modulus G' and the loss modulus G" of the suspension printing support material provided in Example 1 under different shear stresses over time;
[0043] Figure 4 A curve diagram showing the change of storage modulus G' and loss modulus G" of the suspension printing support material provided in Comparative Example 1 over time under different shear stresses;
[0044] Figure 5 This is a grid structure diagram obtained by printing using the suspension printing support material provided in Example 1 as a suspension bath;
[0045] Figure 6 This is a grid structure diagram obtained by using the suspension printing support material provided in Example 2 as a suspension bath printing;
[0046] Figure 7 This is a grid structure diagram obtained by using the suspension printing support material provided in Example 3 as a suspension bath printing;
[0047] Figure 8 This is a grid structure diagram obtained by using the suspension printing support material provided in Comparative Example 1 as a suspension bath printing;
[0048] Fig. 9 A complex letter structure diagram obtained by printing using the suspension printing support material provided in Example 1 as a suspension bath;
[0049] Fig.10 It is a front view of a spiral sphere printed by using the suspension printing support material provided in Example 1 as a suspension bath;
[0050] Fig.11 A top view of a spiral sphere printed using the suspension printing support material provided in Example 1 as a suspension bath;
[0051] Fig.12 Inverted microscope images of HepG2 cells cultured in the suspension printing support material provided in Example 1 on days 0, 1, 3 and 5;
[0052] Fig.13 Inverted microscope images of HepG2 cells cultured in the suspension printing support material provided in Comparative Example 1 on days 0, 1, 3 and 5;
[0053] Fig.14 The cell activity trend diagram of HepG2 cells after being cultured in the suspension printing support material provided in Examples 1 to 3 and Comparative Example 1 for 1, 3 and 5 days;
[0054] Fig.15 The sprouting diagrams are of endothelial cells cultured in the suspension printing support material provided in Example 1 on the first day, one day later, and two days later;
[0055] Fig.16 These are sprouting diagrams of endothelial cells cultured in the suspension printing support material provided in Comparative Example 1 on the first day, one day later, and two days later. DETAILED DESCRIPTION
[0056] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0057] The experimental methods in the following specific implementation modes are all conventional methods unless otherwise specified.
[0058] Unless otherwise specified, the materials, reagents, etc. used in the following specific embodiments can be obtained from commercial sources.
[0059] Some of the raw material information used in the following specific implementations is as follows:
[0060] Methacryloyl collagen (ColMA): purchased from Suzhou Yongqinquan Intelligent Equipment Co., Ltd.;
[0061] Lithium phenyl (2,4,6-trimethylbenzoyl) phosphate (LAP): purchased from Suzhou Yongqinquan Intelligent Equipment Co., Ltd.;
[0062] Nanoclay (XLS): purchased from BYK;
[0063] Phosphate buffer solution (PBS): purchased from Gibco;
[0064] HepG2 cells: purchased from Servicebio;
[0065] HUVEC cells: purchased from Zhongqiao Xinzhou;
[0066] Endothelial cell EGM-2 culture medium kit: purchased from Lonza;
[0067] Gelatin: purchased from Sigma;
[0068] 0.05% trypsin-EDTA and phenol red: purchased from Gibco;
[0069] The composition of HepG2 cell culture medium: including MEM (purchased from Servicebio) and fetal bovine serum (purchased from Sigma) in a volume ratio of 9:1, and 1% penicillin-streptomycin (purchased from Bio-Channel7);
[0070] Cell activity detection reagents: purchased from Novazon Biotechnology.
[0071] Example 1
[0072] A suspension printing support material for supporting cell growth, the preparation method of which comprises the following steps:
[0073] (1) Dissolving methacryloyl collagen (ColMA) and 10X PBS buffer (pH 7.2) in sterile water to obtain a ColMA stock solution with a mass percentage of 10%;
[0074] Dissolve nanoclay (XLS) and 10X PBS buffer (pH 7.2) in sterile water to obtain an XLS mother solution with a mass percentage of 8%;
[0075] (2) The ColMA mother liquor obtained in step (1) and the XLS mother liquor are mixed in a volume ratio of 1:1, and finally 2,4,6-trimethylbenzoyl lithium phosphite (LAP) is added (so that the concentration of LAP is 0.125 g / 100 mL) and mixed thoroughly to obtain the suspended printing support material.
[0076] Embodiment 2-3
[0077] A suspension printing support material for supporting cell growth, which differs from Example 1 in that the mass percentage of XLS in the XLS mother solution in step (1) is 4% (Example 2) and 12% (Example 3), respectively, and other substances, conditions and steps are the same as those in Example 1.
[0078] Comparative Example 1
[0079] A suspension printing support material, the preparation method of which comprises: dissolving ColMA and 10X PBS buffer (pH value is 7.2) in sterile water to obtain ColMA with a mass percentage of 5% and directly using it as the suspension printing support material.
[0080] Performance Test:
[0081] (1) Rheological properties: The rheological properties of the suspended printing support materials were tested at room temperature using an MCR 302 advanced rotational rheometer (Anton Paar, Graz, Austria).
[0082] ① Temperature scanning: When using a parallel plate rotor, the gap between the rotor and the bottom plate of the rheometer needs to be controlled to ensure good contact during the test. When performing the temperature scanning test, a small amount of the material to be tested is added to the center of the lower plate of the rheometer, and then the 405nm blue light is adjusted to irradiate with a light intensity of 20mW and a light exposure time of 20s. After light curing, the rotor is immediately controlled to descend to contact the sample surface to produce a bonding effect, so that the gap between the sample and the lower plate is about 3mm. In the actual process, the gap value can be slightly adjusted according to the actual thickness of the sample to ensure good contact between the sample and the sensor on the rotor. In the oscillating shear scanning mode with a fixed frequency of 1rad / s and a strain of 1%, the heating rate is adjusted to 4℃ / min, and the temperature is set to increase in the range of 0-40℃. The changes in the storage modulus G' and the loss modulus G" with temperature are recorded;
[0083] ② Shear recovery scan: Use similar shear strain changes of 10-1000% to perform shear recovery test. The detailed operation is the same as the temperature scan, and the changes of storage modulus G' and loss modulus G" with time under different shear stresses are recorded;
[0084] The suspension printing support materials provided in Example 1 and Comparative Example 1 were tested according to the above test method. The storage modulus G' and loss modulus G" of the suspension printing support material provided in Example 1 were obtained as a function of temperature. Figure 1 As shown, the storage modulus G' and loss modulus G" of the suspension printing support material provided in Comparative Example 1 vary with temperature as shown in FIG. Figure 2 As shown, the curves of the storage modulus G' and loss modulus G" of the suspension printing support material provided in Example 1 under different stresses over time are shown in FIG. Figure 3 As shown, the curves of the storage modulus G' and loss modulus G" of the suspension printing support material provided in Comparative Example 1 under different stresses over time are shown in FIG. Figure 4 As shown;
[0085] from Figure 1 and Figure 2It can be seen that the suspension printing support material provided in Example 1 has a gel transition point at about 30.06°C, while the suspension printing support material provided in Comparative Example 1 has no gel transition point from beginning to end;
[0086] from Figure 3 and Figure 4 It can be seen that the storage modulus G' and the loss modulus G" of the suspension printing support material provided in Example 1 show periodic changes, indicating that the suspension printing support material provided in Example 1 has shear repair properties, while the storage modulus G' and the loss modulus G" of the suspension printing support material provided in Comparative Example 1 do not show periodic changes, indicating that it has no shear repair properties;
[0087] In summary, it can be explained that the suspension printing support material provided by the present invention has good shear thinning performance and self-supporting performance, can be freely switched between the sol state (low viscosity) and the gel state (high viscosity), and is suitable for use as a suspension bath for suspension printing.
[0088] (2) Suspension printing performance
[0089] ① Add the suspension printing support material into the mold of the suspension printer and place it on the printing platform of the suspension printer; prepare 20% gelatin (the solvent is PBS buffer) and add colored dye (commonly available in the market) and heat it in a 65°C oven to melt and mix well, take an appropriate amount of gelatin solution and add it to the printing barrel as bio-ink for standby use;
[0090] ② Use standard software to generate G code based on the STL file of the 3D model and convey the commands to each layer of printing movement;
[0091] ③ Using a 3D bioprinter with a suspension printing support material as the suspension bath, set the barrel temperature and platform temperature in advance, wait until the suspension bath and bio-ink are balanced to the set temperature, squeeze the bio-ink into the suspension printing support material through a 23G needle with an inner diameter of 25mm and a tube length of 25mm for printing, and produce spiral spheres, grid structures, and complex letter structures;
[0092] Among them, the printer settings when printing the grid structure are as follows: the platform temperature is set to 10°C, the barrel temperature is set to 28°C, the needle tip temperature is set to 28°C, the extrusion speed is 20mm / s, the air pressure is 0.14MPa, the layer height is 0.75mm, and the filling spacing is 1mm;
[0093] The printer settings for printing the spiral sphere structure are as follows: platform temperature is set to 15°C, barrel temperature is set to 28°C, needle tip temperature is set to 28°C, extrusion speed is 4mm / s, air pressure is 0.14MPa, layer height is 1mm, and filling spacing is 1mm;
[0094] The printer settings for printing the letter structure are as follows: platform temperature is set to 15°C, barrel temperature is set to 27°C, needle tip temperature is set to 27°C, extrusion speed is 4mm / s, and air pressure is 0.18MPa;
[0095] According to the above printing method, the suspension printing support materials provided in Examples 1 to 3 and Comparative Example 1 are respectively used as suspension baths for suspension printing. The grid structure obtained by using the suspension printing support materials provided in Examples 1 to 3 as suspension baths is shown in FIG. Figures 5 to 7 As shown, the grid structure obtained by using the suspension printing support material provided in Comparative Example 1 as the suspension bath printing is as shown in Figure 8 As shown; the complex letter structure obtained by using the suspension printing support material provided in Example 1 as the suspension bath printing is as shown Fig. 9 As shown; the front view and top view of the spiral sphere obtained by using the suspension printing support material provided in Example 1 as the suspension bath printing are respectively as shown in Fig.10 and Fig.11 As shown;
[0096] from Figures 5 to 11 It can be seen that the suspended printing support materials provided in Examples 1 to 3 have good printing performance, among which Example 1 has the best printing performance and can support precise grid, curve printing and letter printing, while the suspended printing support material provided in Comparative Example 1 cannot support the printing of precise grid structure, indicating that it is not printable.
[0097] (3) Relative quantitative test of hepG2 cell activity
[0098] ① Cultivate HepG2 cells: Use T75 culture flasks to culture HepG2 cells. Add 8 mL of MEM medium to each T75. Replace the medium every other day. Observe the cell fusion under an inverted microscope and subculture when it reaches 90%. Remove the original medium and rinse the cells with 2 mL of PBS buffer. Add 2 mL of trypsin to each bottle of cells and place them in a 37°C incubator for digestion for 3 minutes before taking them out. After observing the cells fall off at the bottom of the bottle with the naked eye, add 2 mL of MEM medium to stop digestion. Then collect the cells into a 15 mL centrifuge tube (400 g, 5 min), remove the supernatant, resuspend the cells with an appropriate amount of medium, and take 10 μL of the cell suspension for loading on an automatic cell counter to obtain the cell density. The inoculated cell density is 1 to 5×10 6 , calculate the dilution ratio of cells, separate the corresponding volume of cell suspension according to the required cell amount, and centrifuge again;
[0099] ② The suspension printing support material was mixed with HepG2 cells calculated according to the cell density and inoculated into a 96-well cell culture plate. About 5 μL of the mixed cell suspension was added to each well. Under blue light (405 nm), the irradiation energy was 20 mW, and the irradiation time was 20 s. After light curing, 200 μL of cell culture medium was added to each well and placed in a 37°C, 5% carbon dioxide incubator for culture. The cell culture medium was replaced every other day. On the 0th, 1st, 3rd, and 5th days of culture, the cell proliferation was observed under an inverted microscope and photographed and recorded. The cells were then used to detect cell activity experiments;
[0100] ③ Sample preparation for standard curve: Use a cell counter to count the cell density of the hepG2 cell suspension cultured on the day of digestion, and use culture medium to dilute the cell suspension in equal proportions: 10, 10 2 , 10 3 , 10 4 , 10 5 Usually 5 to 7 concentration gradients are required, with 3 replicates in each group. Add each group of cell dilutions to a 96-well plate, add 100 μL of culture medium to each well, and leave at room temperature;
[0101] ④ Prepare the sample to be tested: Take out the cell culture plate to be tested from the incubator in advance and place it at room temperature for 30 minutes to allow the temperature of the culture plate to balance to room temperature. Add CellCounting-Lite 3D of the same volume as the cell culture to be tested and balanced to room temperature. For example, when using a 96-well culture plate, pipette 100μL CellCounting-Lite3D into 100μL of the cell culture to be tested, and shake vigorously for 5 minutes to fully lyse the cell clusters. The cell lysis step in this experimental process can be placed on a horizontal shaker in the dark and shaken for 2 hours to stabilize the luminescent signal before detection.
[0102] ⑤ Create a standard curve. According to the known cell amount and the luminescence detection value of the corresponding group, create a standard curve with the cell number as the X-axis coordinate and the luminescence value as the Y-axis coordinate. Calculate the number of live cells in each group of the experimental data of the day based on the standard curve for each day, and perform statistical analysis on the live cell number data for three days.
[0103] The suspension printing support materials provided in Examples 1 to 3 and Comparative Example 1 were tested according to the above test method. The inverted microscope images of HepG2 cells cultured in the suspension printing support material provided in Example 1 on days 0, 1, 3 and 5 were obtained as shown in FIG. Fig.12 As shown, the inverted microscope images of HepG2 cells cultured in the suspension printing support material provided in Comparative Example 1 on days 0, 1, 3 and 5 are shown in FIG. Fig.13As shown, the cell activity trend diagrams of HepG2 cells cultured in the suspension printing support materials provided in Examples 1 to 3 and Comparative Example 1 after 1, 3 and 5 days are obtained by calculation as shown in FIG. Fig.14 As shown;
[0104] from Figures 12-14 It can be seen that the suspension printing support materials provided in Examples 1 to 3 have good biological activity and support continuous cell growth, which is not much different from the cell activity in the suspension printing support material provided in Comparative Example 1, indicating that the addition of nanoclay will not affect cell activity.
[0105] (4) Endothelial cell sprouting experiment
[0106] ① Culture of vascular endothelial cells (HUVEC): Use T75 culture flasks to culture HUVEC cells. Add 8 mL of EGM-2 medium to each T75. Change the medium every day. Use an inverted microscope to observe that the cells are 90% confluent and can be passaged. Remove the original medium and rinse the cells with 2 mL of PBS buffer. Add 2 mL of trypsin to each bottle of cells and place them in a 37°C incubator for digestion for 3 minutes before taking them out. After observing that the cells at the bottom of the bottle fall off with the naked eye, add 2 mL The digestion was terminated with EGM-2 medium, and then the cells were collected into a 15 mL centrifuge tube (400 g, 5 min), the supernatant was removed, and the cells were resuspended with an appropriate amount of medium, and 10 μL of the cell suspension was used for loading on an automatic cell counter to obtain the cell density; the dilution ratio was calculated according to the cell density, and the cell suspension was inoculated along the well wall into a pre-treated 96-well transparent round-bottom ultra-low adsorption microplate, with about 200 cells per well, and the total volume was supplemented with cell culture medium to about 100 μL per well. The culture plate should not be shaken violently or cultured with vibration, which would destroy the ultra-low adsorption hydrogel and cause the cells to fail to form agglomerates; the culture plate with cells was placed in a 37° C., 5% carbon dioxide incubator for culture, and generally, agglomerates began to form after 12 hours;
[0107] ② Agglomeration experiment: Prepare suspension printing materials as precursor solutions, take endothelial cell spheres that have aggregated within 12 to 24 hours of culture and mix them into the precursor solution, then take 500 μL of the precursor solution containing the cell spheres and add it to the cell culture dish. After solidification by irradiation with blue light for 20 seconds, add 1 mL of culture medium to each dish, and then culture in a 37°C, 5% carbon dioxide incubator. Change the culture medium every day, and observe the budding of the endothelial cell spheres under an inverted microscope on the 1st and 2nd day of culture and take photos for record.
[0108] The suspension printing support materials provided in Example 1 and Comparative Example 1 were tested according to the above test method. The budding patterns of endothelial cells cultured in the suspension printing support materials provided in Example 1 on the first day, after 1 day of culture, and after 2 days of culture were obtained as shown in the figure below. Fig.15As shown, the sprouting diagrams of endothelial cells cultured in the suspension printing support material provided in Comparative Example 1 on the first day, after 1 day of culture, and after 2 days of culture are shown in FIG. Fig.16 As shown;
[0109] from Fig.15 and 16 It can be seen that the suspension printing support material provided in Example 1 has good vascularization activity and supports the spontaneous sprouting of endothelial cells in Example 1.
[0110] The applicant declares that the present invention illustrates a suspension printing support material supporting cell growth and its preparation method and application through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A suspension printing support material suitable for constructing large-scale hierarchical vascularized organs as a suspension bath supporting cell growth, characterized in that: The suspension printing support material includes a bio-based polymer and an inorganic nano-material; the mass ratio of the bio-based polymer to the inorganic nano-material is 10:(4-12); The bio-based polymer is methacryloyl collagen; The inorganic nanomaterial includes nanoclay; The suspension printing support material also includes a photoinitiator.
2. The suspension printing support material according to claim 1, characterized in that: The photoinitiator is a biocompatible photoinitiator.
3. The suspension printing support material according to claim 2, characterized in that: The biocompatible photoinitiator includes a biocompatible ultraviolet light initiator or a biocompatible visible light initiator.
4. The suspension printing support material according to claim 3, characterized in that: The biocompatible ultraviolet light initiator includes 2-hydroxy-4-(2-hydroxyethoxy)-2-methylpropiophenone and / or ethyl 2,4,6-trimethylbenzoylphenylphosphonate.
5. The suspension printing support material according to claim 3, characterized in that: The biocompatible visible light initiator includes lithium phenyl-2,4,6-trimethylbenzoylphosphinate.
6. A method for preparing a suspension printing support material according to any one of claims 1 to 5, characterized in that: The preparation method comprises: mixing a bio-based polymer, an inorganic nanomaterial and a photoinitiator in a solvent to obtain the suspended printing support material.
7. An artificial vascularized organ, characterized in that: The artificial vascularized organ is obtained by suspension printing using the suspension printing support material and cells as described in any one of claims 1 to 5.
8. The artificial vascularized organ according to claim 7, characterized in that: The cells include endothelial cells, fibroblasts, induced pluripotent stem cells, HepG2 cells, A549 cells, 293 cells, Hela cells, MCF7 cells, CHO-K1 cells, mesenchymal stem cells, smooth muscle cells, hematopoietic stem cells, and any one or a combination of at least two of primary cells extracted from the brain, heart, liver, kidney, intestine, stomach, reproductive organs or muscle tissue organs.
9. The artificial vascularized organ according to claim 7, characterized in that: The biological ink used in the suspension printing includes any one of gelatin, hydroxyapatite, polylactic acid or polylactic acid-co-lactic acid, or a combination of at least two thereof.
10. A method for preparing an artificial vascularized organ according to any one of claims 7 to 9, characterized in that: The preparation method comprises the following steps: (1) adding cells to the suspension printing support material according to any one of claims 1 to 5 to obtain a suspension bath containing cells; (2) Using biological ink to perform suspension printing in the cell-containing suspension bath obtained in step (1), and after curing, obtaining the artificial vascularized organ.
11. The preparation method according to claim 10, characterized in that: The curing in step (2) is photocuring or thermal curing.
12. The preparation method according to claim 11, characterized in that: The intensity of the light curing is 5-30 mW / cm 2 .
13. The preparation method according to claim 11, characterized in that: The light curing time is 10 to 60 s.
14. Use of the artificial vascularized organ according to any one of claims 7 to 9 in organogenesis research, organ pathology research or drug screening research.
Citation Information
Patent Citations
Suspension medium for suspension 3D biological printing and preparation method and application thereof
CN114854042A
Nanocomposite Ionic-Covalent Entanglement Reinforcement Mechanism and Hydrogel
US20200071550A1
Bioink and crosslinkable support medium for printing
US20210154368A1