A method for thermal cracking and hydrogenation refining of waste plastics

By using a gas-phase slurry bed reactor and a fixed-bed dechlorination reactor for refining treatment in a hydrogen environment, the problem of impurities in cracked gas and oil during the thermal cracking of waste plastics is solved, achieving efficient recycling and the production of high-quality raw materials. production, solving the problems of resource waste and carbon emissions in the existing technology.

CN117801838BActive Publication Date: 2024-10-18SHANGHAI PHELIX NEW MATERIALS CO LTD

Patent Information

Application Number
CN202311872569.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-10-18
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

In the existing technology, the pyrolysis gas generated by the thermal cracking process of waste plastics cannot be directly used in industrial production, resulting in a large amount of carbon emissions and resource waste. Moreover, the impurities in the waste plastic oil affect the subsequent processing technology, making it difficult to achieve efficient recycling.

Method used

In a hydrogen environment, olefin saturation, denitrification, desulfurization and dechlorination reactions are carried out through a gas phase slurry bed reactor and a fixed bed dechlorination reactor, combined with a hydrogenation catalyst and dechlorination agent, to refine waste plastic cracking gas and oil, reducing Impurity content, resulting in high quality feedstock for steam cracking.

Benefits of technology

It achieves efficient chemical recycling of waste plastics, reduces the cost of hydrogenation equipment, improves the quality of cracked oil, meets the feed requirements of steam cracking, and reduces carbon emissions and resource waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117801838B_ABST
    Figure CN117801838B_ABST
Patent Text Reader

Abstract

The invention belongs to the field of petrochemical industry, and discloses a method and device for the hydrogenation pyrolysis of mixed waste plastics and the refining of pyrolysis products. The mixed waste plastics are pyrolyzed in a hydrogen environment to generate plastic pyrolysis gas and plastic pyrolysis oil, the pyrolysis gas contacts the catalyst, the pyrolysis gas is first hydrogenated and saturated in a slurry bed reactor, and then dechlorinated in a dechlorination reactor; the pyrolysis oil is successively subjected to a pre-hydrogenation reaction, a refining main reaction and a dechlorination reactor, and contacts the catalyst under reaction conditions. The refined reaction products of the waste plastic pyrolysis gas and the pyrolysis oil are passed through a fractionation system to obtain saturated dry gas and liquefied gas, light oil products and hydrogenated tail oil; the saturated liquefied gas, light oil products and hydrogenated tail oil can directly enter different raw material ports of an ethylene steam cracking furnace. The invention can effectively remove impurities in waste plastic oil and waste plastic pyrolysis gas, provide high-quality pyrolysis raw materials for the steam cracking preparation process, truly realize the full circulation of waste plastics, and the device has low operating costs and a long operating cycle. The invention is suitable for the recycling of waste plastics and is used to prepare high-quality ethylene pyrolysis raw materials from waste plastics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of petrochemical industry and relates to a waste plastic cracking and cracking product hydrogenation system. Background Art

[0002] Plastics are now ubiquitous in our lives, from beverage bottles and disposable straws to children's toys, clothes hangers, and shopping bags. Plastics now account for 15% to 20% of existing municipal solid waste, much of which is single-use plastic packaging. This has led to a surge in the use of single-use plastics, threatening international environmental standards and causing various social problems. Disposing of mixed plastic waste is challenging. Recently, pyrolysis and chemical conversion of waste plastics have attracted interest in treating plastic waste and reducing greenhouse gas emissions from incineration.

[0003] Chemical conversion methods can transform plastic waste into valuable industrial raw materials or fuel oil, eliminating environmental pollution while also achieving sustainable resource utilization, making it an effective way to combat "white pollution." Currently, the waste plastics refining industry is flourishing in China, with some companies already having built small-scale pyrolysis units. However, the high-value utilization of waste plastics pyrolysis products remains to be effectively addressed.

[0004] Waste plastic oils converted through various processes differ significantly from traditional petroleum-based oils. They contain high levels of impurities, particularly chlorine and silicon, which significantly complicate subsequent processing. Currently, little research has been conducted on the deep processing of waste plastic oils. Many studies have focused on the impact of chlorine impurities in waste plastic oils on their subsequent processing, ignoring the fact that waste plastic oils also contain other impurities, such as silicon and metal impurities, and the significant impact these impurities can have on subsequent processing.

[0005] Among them, numerous patents, such as CN101724426B, CN102942951A, CN102226103A, CN104726134A, and CN104611060A, disclose various technologies, including olefin saturation and impurity removal, for producing clean fuel from waste plastic oil. From the perspective of plastic recycling, and especially carbon emissions, products produced by hydrogenating waste plastics to fuel oil ultimately end up in combustion, accompanied by significant greenhouse gas emissions. Hydrogenating waste plastics to fuel oil is considered incompatible with the concept of sustainable development.

[0006] The thermal cracking process of waste plastics produces approximately 15% pyrolysis gas. In existing technologies, due to the complex composition of pyrolysis gas and its inability to be directly used as industrial raw materials, the pyrolysis gas can only be directly burned to recover heat. Direct combustion of pyrolysis gas not only causes significant material losses in the waste plastics recycling process, but also leads to large amounts of carbon emissions, significantly reducing the economic and environmental benefits of chemical recycling of waste plastics. The pyrolysis gas is primarily composed of hydrogen and unsaturated liquefied gas components. After being refined and purified by the method provided by the present invention, the hydrogen and methane enter the hydrogen production unit to produce hydrogen, C2, and liquefied gas components, which can directly serve as cracking feedstock for the ethylene cracking unit. Summary of the Invention

[0007] In order to solve the above deficiencies in the prior art, the present invention aims to provide a hydrogenation system for hydrogenated waste plastic cracking products, so as to achieve the purpose of fully recycling polyolefin waste plastics.

[0008] To achieve the above object, the technical solutions adopted by the present invention are as follows:

[0009] A waste plastic hydrocracking and cracking product hydrogenation system,

[0010] The specific steps include:

[0011] S1. In a hydrogen environment, waste plastics are thermally cracked to generate waste plastic cracking oil and gas;

[0012] S2. Under a hydrogen environment, the waste plastic cracking gas passes through a gas phase slurry bed reactor and a fixed bed dechlorination reactor in sequence, and undergoes olefin saturation, denitrification, desulfurization and dechlorination reactions under the action of a hydrogenation catalyst and a dechlorination agent to obtain refined waste plastic cracking gas;

[0013] S3, under a hydrogen environment, the waste plastic pyrolysis oil passes through a pre-hydrogenation reactor, a refining reactor and a dechlorination reactor in sequence, and undergoes diene saturation, demetallization, desiliconization, denitrogenation, olefin saturation and dechlorination reactions under the action of a hydrogenation catalyst and a dechlorinating agent to obtain refined waste plastic pyrolysis oil;

[0014] S4, refined oil and refined gas are distilled into dry gas, saturated liquefied gas, light oil and hydrogenated tail oil; the silicon content of the gas and liquid phase materials in the obtained reaction effluent is less than 0.5μg / g, the chlorine content is less than 0.3μg / g, and the metal content is less than 1μg / g;

[0015] As a limitation of the present invention, the reaction temperature in the gas phase slurry bed reactor in S2 is 150° C. to 250° C., and the pressure in the reactor is 1 MPa to 2 MPa;

[0016] As another limitation of the present invention, the hydrogenation catalyst in S2 and S3 is a composite molecular sieve-supported Ni-Mo series catalyst, wherein the molecular sieve is a hydrogen-type all-silicon MCM-41 and / or HY type molecular sieve; the molar ratio of Ni to Mo in the catalyst is 1.5-3.5:2-17;

[0017] As a third limitation of the present invention, the waste plastic oil is a hydrocarbon material obtained by converting waste plastics through at least one of catalytic cracking, catalytic cracking, and dissolution liquefaction; the waste plastic oil has a distillation range of 50-550°C, a silicon content of less than 5000 μg / g, a chlorine content of less than 5000 μg / g, and a metal content of less than 5000 μg / g; the composition of the waste plastic oil includes an olefin volume fraction of 5-80%, preferably 5-60%, an aromatic hydrocarbon volume fraction of less than 90%, preferably 2-40%, and a paraffin volume fraction of less than 90%, preferably 5-60%;

[0018] Catalytic cracking and catalytic cracking reactions refer to the decomposition of hydrocarbon-based waste plastics into smaller molecules under high temperature conditions and in the presence of a catalyst. Depending on the reaction products, reactions that produce low-carbon olefins (ethylene, propylene, butene) are called catalytic cracking reactions, while reactions that produce motor gasoline are called catalytic cracking reactions.

[0019] Dissolution-liquefaction reaction refers to the reaction in which waste plastics are converted from solid to liquid in the presence of solvent oil and / or organic solvent;

[0020] As a fourth limitation of the present invention, the dechlorination reaction catalyst described in S2 and S3 has a carrier of aluminum oxide, a butterfly shape, an equivalent diameter of 1.6 mm, and a composition comprising: 10 wt.% of sodium carbonate, 3.5 wt.% of magnesium oxide, and 8.0 wt.% of calcium;

[0021] As a fifth limitation of the present invention, the reaction temperature of the hydrogenation reaction in S2 is 150° C. to 250° C., and the pressure is 1 MPa to 2 MPa;

[0022] As a sixth limitation of the present invention, the reaction temperature of the dechlorination reaction in S2 is 150° C. to 250° C., and the pressure is 1 MPa to 2 MPa;

[0023] The present invention has no restrictions on the shape of the hydrogenation catalyst. For example, the shape includes spherical, clover-shaped, butterfly-shaped, Raschig ring, honeycomb and other various special shapes. Even for the catalyst in the slurry bed reactor, its appearance is powdery.

[0024] The dechlorination agent comprises at least one Group IA metal compound and / or at least one Group IIA metal compound, optionally one or more metal oxides selected from Ca, Cu, Fe, Zn, and a carrier and / or a binder;

[0025] The carrier and / or binder is selected from one or more of silica, alumina, silica-alumina, zirconia, and clay. The clay is selected from one or more of kaolin, illite, montmorillonite, and bentonite; the kaolin includes halloysite.

[0026] In the present invention, "optional" means optional, and the optional one or more metal oxides selected from Ca, Cu, Fe, and Zn means that the one or more metal oxides selected from Ca, Cu, Fe, and Zn are optional components of the dechlorination agent;

[0027] In the present invention, under preferred circumstances, the dechlorination agent is a high-temperature dechlorination agent and / or a medium-temperature dechlorination agent. The present invention has no limitation on high-temperature dechlorination agents and medium-temperature dechlorination agents, and conventional high-temperature dechlorination agents and medium-temperature dechlorination agents can achieve the present invention;

[0028] Further preferred are high-temperature dechlorination agents and / or medium-temperature dechlorination agents having a larger chlorine capacity;

[0029] As a seventh limitation of the present invention, the waste plastic is at least one of waste plastic in fresh domestic waste, waste plastic in industrial and agricultural production, and waste plastic in aged waste, and the type of the waste plastic is at least one selected from PE, PP, PS, and PVC;

[0030] As an eighth limitation of the present invention, the hydrogenation catalyst and the dechlorination agent are uniformly mixed and loaded or loaded in layers, and along the direction of material flow, the equivalent diameter of the hydrogenation catalyst gradually decreases, the pore size gradually decreases, and the active metal content gradually increases; or they are dispersed in a slurry bed solvent in a suspended state; the loading volume ratio of the dechlorination agent to the catalyst is 1 to 90:35 to 120;

[0031] In one embodiment of the present invention, the de-doping reaction (i.e., dechlorination, desiliconization, and demetallation) is carried out under the following conditions: hydrogen partial pressure of 0.5-20.0 MPa, reaction temperature of 250-300°C, volume space velocity of 0.1-30 h -1 , Hydrogen to oil volume ratio 5~1000Nm 3 / m 3 ;

[0032] In the hydrofining reaction process of the present invention, the reaction effluent obtained from the impurity removal step directly enters the hydrofining reactor, and under the hydrofining reaction conditions, it contacts and reacts with the hydrofining catalyst to remove impurities such as sulfur and nitrogen, and hydrogenate and saturate the olefins;

[0033] The reaction effluent from the hydrotreating reactor is separated to produce a gaseous phase and a liquid phase. In one embodiment of the present invention, the resulting liquid phase has an olefin content of ≤2 wt.%, a sulfur content of <50 μg / g, a nitrogen content of <50 μg / g, a silicon content of <1 μg / g, a chlorine content of <0.5 μg / g, and a metal content of <1 μg / g. The resulting liquefied gas component and refined oil liquid phase are low in sulfur, nitrogen, and olefins, and all or part of them can be used as cracking feedstock for steam cracking to produce ethylene.

[0034] Due to the adoption of the above technical solution, the present invention has the following beneficial effects compared with the prior art:

[0035] (1) The hydrogen pyrolysis and hydrogenation refining method of waste plastics provided by the present invention provides a highly efficient chemical recycling method for waste plastics, mainly polyolefins. The consumption ratio of polyolefin plastics accounts for more than 80% of the five major general-purpose plastics. This solves the recycling problem of polyolefin waste plastics and can effectively solve the problem of white pollution.

[0036] (2) The method for hydrogenation and refining of waste plastics provided by the present invention uses the plastic cracking dry gas to produce hydrogen to achieve self-sufficiency in hydrogen source for hydrogenation of waste plastic cracking oil, thus achieving high-value utilization of waste plastic cracking gas while effectively reducing the operating cost of the hydrogenation device;

[0037] (3) The method for hydrogenation and hydrogenation refining of waste plastics provided by the present invention solves the chemical cycle of waste plastic cracking gas. Waste plastic cracking gas accounts for 15%-20% of plastic cracking products. Since the gas contains a large amount of organic chlorides, organic silicon, sulfides, organic nitrogen, unsaturated hydrocarbons, etc., it cannot be directly sent to the downstream for utilization. The previous technology is to directly burn it, which causes a large amount of material loss and may bring great environmental pollution. The present invention adopts a gas-phase slurry bed reactor to select catalysts and realizes the resource utilization of waste plastic cracking gas at relatively low temperatures and pressures such as 150℃~250℃ and 1MPa~2MPa;

[0038] (4) The method for hydrogen pyrolysis and hydrogenation refining of waste plastics provided by the present invention is aimed at a type of highly polluted waste plastic with high silicon and high chlorine content. After thermal cracking and hydrogenation treatment by this method, it meets the feed requirements of steam cracking and realizes closed-loop plastic recycling;

[0039] (5) The method for hydrogenation and hydrorefining of waste plastics provided by the present invention significantly improves the quality of the cracked oil produced. Steam cracking units pursue greater yields of ethylene, propylene, and butene. The product of the present invention provides a new cracking raw material for steam cracking units, which has better cracking performance than commercially available naphtha and hydrogenated tail oil, and can obtain a greater yield of light olefins;

[0040] (6) The present invention provides a method for the hydrogenation and hydrorefining of waste plastics. Based on the poor quality of waste plastic oil, a method is proposed to meet the requirements of steam cracking feed after hydrogenation, so that the recycling of plastics can be closed;

[0041] (7) The method for hydrogen pyrolysis and hydrorefining of waste plastics provided by the present invention improves the yield of pyrolysis oil and avoids excessive cracking of light fractions by hydrorefining only the pyrolysis oil, thereby maximizing the overall target product yield;

[0042] (8) The method for hydrogen pyrolysis and hydrogenation refining of waste plastics provided by the present invention avoids isomerization and cyclization reactions by only hydrogenating the pyrolysis oil, thereby reducing the BMCI value of the pyrolysis oil product and obtaining higher steam cracking performance.

[0043] In summary, the waste plastic crude cracking oil and gas hydrogenation system provided by the present invention can effectively remove impurities in waste plastic oil and gas, provide high-quality cracking raw materials for the subsequent steam cracking process, and has low cost and long operation cycle.

[0044] The present invention is suitable for recycling and processing waste plastics and is used for preparing cracking oil and gas by cracking the waste plastics. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] The present invention will be described in further detail below with reference to the accompanying drawings and specific embodiments.

[0046] Figure 1 It is a schematic diagram of one embodiment of the method for hydrogen thermal cracking and hydrogenation refining of waste plastics provided by the present invention.

[0047] In the figure: 1. Hydrogenation thermal cracking reactor; 2. Booster pump; 3. Heat exchanger and heating furnace; 4. Pre-hydrogenation protection reactor; 5. Refining reactor; 6. Dechlorination reactor; 7. Gas-liquid separation tank; 8. Circulating hydrogen compressor; 9. Distillation tower; 10. Gas-phase fixed-bed dechlorination reactor; 11. Gas-phase slurry-bed hydrogenation reactor; 12. Slurry circulation pump; A. Material movement route; B. Hydrogen operation route; M. Pressure gauge. DETAILED DESCRIPTION

[0048] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and understand the present invention and are not intended to limit the present invention.

[0049] Example 1 A method for thermal cracking and hydrogenation refining of waste plastics

[0050] Figure 1 This is a schematic diagram of one embodiment of the method for hydrogen pyrolysis and hydrogenation refining of waste plastics provided by the present invention, as shown in FIG. Figure 1As shown; first, the circulating hydrogen compressor 8 is turned on, so that the hydrogen starts to circulate along the hydrogen running route B;

[0051] The method for hydrogen pyrolysis and hydrogenation refining of waste plastics involved in the present invention specifically comprises the following steps:

[0052] S1, under hydrogen environment, the mixed waste plastic high-pressure melt is introduced into the hydrogen thermal cracking reactor along the material movement route A, and is subjected to thermal cracking reaction with hydrogen at a reactivity of 450°C and an internal pressure of 1.6MPa to generate waste plastic cracking oil and gas, which is then flowed into the gas-liquid separator 7 for gas-liquid separation to obtain waste plastic cracking gas and waste plastic cracking oil respectively;

[0053] S2, the waste plastic cracking gas enters the gas phase slurry bed hydrogenation reactor 11 along the pipeline, and undergoes hydrogenation reaction under the conditions of a reaction temperature of 150° C. and a pressure of 1.4 MPa, wherein the hydrogen is 30% in excess of the total amount of the mixed olefin components. The unreacted slurry is re-introduced into the gas phase slurry bed hydrogenation reactor 11 through the slurry circulation pump 12 for continuous hydrogenation reaction. The gas phase hydrogenated saturated gas obtained enters the gas phase fixed bed dechlorination reactor through the pipeline, and undergoes dechlorination reaction under the conditions of 250° C. and 1.4 MPa. The obtained refined gas is introduced into the distillation tower 9 for rectification;

[0054] S3, under the protection of circulating hydrogen, the waste plastics pyrolysis oil is earlier through booster pump 2, and is heated through heat exchanger and heating furnace 3 with circulating hydrogen again, the mixed hydrogen material after the heating is 300 ℃ at reaction temperature through pre-hydrogenation protection reactor 4, refining reactor 5 and dechlorination reactor 6 successively, and pressure is under the condition of 5MPa, carry out removing assorted reaction, remove the metallic impurities existing in the plastics pyrolysis oil, as: sodium, calcium and semi-metallic silicon, arsenic and non-metallic sulphur, chlorine, nitrogen, oxygen etc. are removed;

[0055] The refined oil obtained after the impurity removal reaction enters the gas-liquid separation tank through a pipeline to separate excess hydrogen and refined oil. The hydrogen is recycled back to the circulating hydrogen compressor 8, and the refined oil flows into the distillation tower 9 through a pipeline;

[0056] S4, the refined oil and refined gas are distilled and separated at 350 ° C in the distillation tower 9, and the dry gas and liquefied gas are fried and extracted from the top of the distillation tower 9; the light cracking oil with a final boiling point of less than 350 ° C flows out of the distillation port of the distillation tower 9; the saturated liquefied gas and oil products with a final boiling point of less than 350 ° C flowing out of the top of the tower are high-quality steam cracking raw materials, which are suitable for most commercial steam cracking furnaces;

[0057] The oil with a fraction greater than 350°C is extracted from the bottom of the fractionating tower. The refined oil with a fraction greater than 350°C is hydrogenated tail oil, which has a chemical composition of saturated alkanes and has good ethylene cracking performance. It is a high-quality ethylene cracking material and can be used as a feedstock for ethylene cracking furnaces with heavy feedstock acceptance capacity.

[0058] The hydrogenation catalyst used in the hydrogenation reaction of S2 and S3 is a composite molecular sieve-supported Ni-Mo series catalyst, the molecular sieve uses hydrogen-type all-silicon MCM-41 and / or HY type molecular sieve, and the molar ratio of Ni to Mo in the catalyst is 1.5:2;

[0059] The silicon content of the gas-liquid phase materials in the obtained reaction effluent is less than 0.5 μg / g, the chlorine content is less than 0.3 μg / g, and the metal content is less than 1 μg / g.

[0060] Example 2 A method for thermal cracking and hydrogenation refining of waste plastics

[0061] First, the circulating hydrogen compressor 8 is turned on, so that the hydrogen begins to circulate along the hydrogen running route B;

[0062] The method for hydrogen pyrolysis and hydrogenation refining of waste plastics involved in the present invention specifically comprises the following steps:

[0063] S1, under hydrogen environment, the mixed waste plastic high-pressure melt is introduced into the hydrogen thermal cracking reactor along the material movement route A, and is subjected to thermal cracking reaction with hydrogen at a reactivity of 400°C and an internal pressure of 1MPa to generate waste plastic cracking oil and gas, which is then flowed into the gas-liquid separator 7 for gas-liquid separation to obtain waste plastic cracking gas and waste plastic cracking oil respectively;

[0064] S2, the waste plastic cracking gas enters the gas phase slurry bed hydrogenation reactor 11 along the pipeline, and undergoes hydrogenation reaction under the conditions of reaction temperature of 250° C. and pressure of 1 MPa, wherein hydrogen is 30% in excess of the total amount of the mixed olefin components. The unreacted slurry is re-introduced into the gas phase slurry bed hydrogenation reactor 11 through the slurry circulation pump 12 for continuous hydrogenation reaction. The gas phase hydrogenated saturated gas obtained enters the gas phase fixed bed dechlorination reactor through the pipeline, and undergoes dechlorination reaction under the conditions of 150° C. and 1 MPa. The obtained refined gas is introduced into the distillation tower 9 for rectification;

[0065] S3, under the protection of circulating hydrogen, the waste plastics pyrolysis oil is earlier through booster pump 2, and is heated through heat exchanger and heating furnace 3 with circulating hydrogen again, the mixed hydrogen material after the heating is 300 ℃ at reaction temperature through pre-hydrogenation protection reactor 4, refining reactor 5 and dechlorination reactor 6 successively, and pressure is under the condition of 8MPa, carry out removing assorted reaction, remove the metallic impurities existing in the plastics pyrolysis oil, as: sodium, calcium and semi-metallic silicon, arsenic and non-metallic sulphur, chlorine, nitrogen, oxygen etc. are removed;

[0066] The refined oil obtained after the impurity removal reaction enters the gas-liquid separation tank through a pipeline to separate excess hydrogen and refined oil. The hydrogen is recycled back to the circulating hydrogen compressor 8, and the refined oil flows into the distillation tower 9 through a pipeline;

[0067] S4, the refined oil and refined gas are distilled and separated at 350 ° C in the distillation tower 9, and the dry gas and liquefied gas are extracted from the top of the distillation tower 9; the light cracking oil with a final boiling point of less than 350 ° C flows out of the distillation port of the distillation tower 9; the saturated liquefied gas and oil products with a final boiling point of less than 350 ° C flowing out of the top of the tower are high-quality steam cracking raw materials, which are suitable for most commercial steam cracking furnaces;

[0068] The oil with a fraction greater than 350°C is extracted from the bottom of the fractionating tower. The refined oil with a fraction greater than 350°C is hydrogenated tail oil, which has a chemical composition of saturated alkanes and has good ethylene cracking performance. It is a high-quality ethylene cracking material and can be used as a feedstock for ethylene cracking furnaces with heavy feedstock acceptance capacity.

[0069] Among them, the hydrogenation catalyst used in the hydrogenation reaction of S2 and S3 is a composite molecular sieve-loaded Ni-Mo series catalyst, the molecular sieve uses hydrogen-type all-silicon MCM-41 molecular sieve, and the molar ratio of Ni and Mo in the catalyst is 3.5:2.

[0070] The silicon content of the gas-liquid phase materials in the reaction effluent is less than 0.5 μg / g, the chlorine content is less than 0.3 μg / g, and the metal content is less than 1 μg / g.

[0071] Example 3 A method for thermal cracking and hydrogenation refining of waste plastics

[0072] First, the circulating hydrogen compressor 8 is turned on, so that the hydrogen begins to circulate along the hydrogen running route B;

[0073] The method for hydrogen pyrolysis and hydrogenation refining of waste plastics involved in the present invention specifically comprises the following steps:

[0074] S1, under hydrogen environment, the mixed waste plastic high-pressure melt is introduced into the hydrogen thermal cracking reactor along the material movement route A, and is subjected to thermal cracking reaction with hydrogen at a reactivity of 500 ° C and an internal pressure of 1.3 MPa to generate waste plastic cracking oil and gas, and is made to flow into the gas-liquid separator 7 for gas-liquid separation to obtain waste plastic cracking gas and waste plastic cracking oil respectively;

[0075] S2, the waste plastic cracking gas enters the gas phase slurry bed hydrogenation reactor 11 along the pipeline, and undergoes hydrogenation reaction under the conditions of reaction temperature of 250° C. and pressure of 1 MPa, wherein hydrogen is 30% in excess of the total amount of the mixed olefin components. The unreacted slurry is re-introduced into the gas phase slurry bed hydrogenation reactor 11 through the slurry circulation pump 12 for continuous hydrogenation reaction. The gas phase hydrogenated saturated gas obtained enters the gas phase fixed bed dechlorination reactor through the pipeline, and undergoes dechlorination reaction under the conditions of 250° C. and 1 MPa. The obtained refined gas is introduced into the distillation tower 9 for rectification;

[0076] S3, under the protection of circulating hydrogen, the waste plastics pyrolysis oil is earlier through booster pump 2, and is heated through heat exchanger and heating furnace 3 with circulating hydrogen again, the mixed hydrogen material after the heating is 300 ℃ at reaction temperature through pre-hydrogenation protection reactor 4, refining reactor 5 and dechlorination reactor 6 successively, and pressure is under the condition of 8MPa, carry out removing assorted reaction, remove the metallic impurities existing in the plastics pyrolysis oil, as: sodium, calcium and semi-metallic silicon, arsenic and non-metallic sulphur, chlorine, nitrogen, oxygen etc. are removed;

[0077] The refined oil obtained after the impurity removal reaction enters the gas-liquid separation tank through a pipeline to separate excess hydrogen and refined oil. The hydrogen is recycled back to the circulating hydrogen compressor 8, and the refined oil flows into the distillation tower 9 through a pipeline;

[0078] S4, the refined oil and refined gas are distilled and separated at 350 ° C in the distillation tower 9, and the dry gas and liquefied gas are extracted from the top of the distillation tower 9; the light cracking oil with a final boiling point of less than 350 ° C flows out of the distillation port of the distillation tower 9; the saturated liquefied gas and oil products with a final boiling point of less than 350 ° C flowing out of the top of the tower are high-quality steam cracking raw materials, which are suitable for most commercial steam cracking furnaces;

[0079] The oil with a fraction greater than 350°C is extracted from the bottom of the fractionating tower. The refined oil with a fraction greater than 350°C is hydrogenated tail oil, which has a chemical composition of saturated alkanes and has good ethylene cracking performance. It is a high-quality ethylene cracking material and can be used as a feedstock for ethylene cracking furnaces with heavy feedstock acceptance capacity.

[0080] The hydrogenation catalyst used in the hydrogenation reaction of S2 and S3 is a composite molecular sieve-supported Ni-Mo series catalyst, the molecular sieve uses HY type molecular sieve, and the molar ratio of Ni to Mo in the catalyst is 1.5:17.

[0081] The silicon content of the gas and liquid phase materials in the reaction effluent is less than 0.5μg / g, the chlorine content is less than 0.3μg / g, and the metal content is less than 1μg / g

[0082] Example 4 A method for thermal cracking and hydrogenation refining of waste plastics

[0083] First, the circulating hydrogen compressor 8 is turned on, so that the hydrogen begins to circulate along the hydrogen running route B;

[0084] The method for hydrogen pyrolysis and hydrogenation refining of waste plastics involved in the present invention specifically comprises the following steps:

[0085] S1, under hydrogen environment, the mixed waste plastic high-pressure melt is introduced into the hydrogen thermal cracking reactor along the material movement route A, and is subjected to thermal cracking reaction with hydrogen at a reactivity of 400°C and an internal pressure of 2MPa to generate waste plastic cracking oil and gas, which is then flowed into the gas-liquid separator 7 for gas-liquid separation to obtain waste plastic cracking gas and waste plastic cracking oil respectively;

[0086] S2, the waste plastic cracking gas enters the gas phase slurry bed hydrogenation reactor 11 along the pipeline, and undergoes hydrogenation reaction under the conditions of a reaction temperature of 150° C. and a pressure of 2 MPa, wherein the hydrogen is 30% in excess of the total amount of the mixed olefin components. The unreacted slurry is re-introduced into the gas phase slurry bed hydrogenation reactor 11 through the slurry circulation pump 12 for continuous hydrogenation reaction. The gas phase hydrogenated saturated gas obtained enters the gas phase fixed bed dechlorination reactor through the pipeline, and undergoes dechlorination reaction under the conditions of 250° C. and 2 MPa. The obtained refined gas is introduced into the distillation tower 9 for rectification;

[0087] S3, under the protection of circulating hydrogen, the waste plastics pyrolysis oil is earlier through booster pump 2, and is heated through heat exchanger and process furnace 3 with circulating hydrogen again, the mixed hydrogen material after the heating is 250 ℃ at reaction temperature through pre-hydrogenation protection reactor 4, refining reactor 5 and dechlorination reactor 6 successively, and pressure is under the condition of 5MPa, carry out removing assorted reaction, remove the metallic impurities existing in the plastics pyrolysis oil, as: sodium, calcium and semi-metallic silicon, arsenic and non-metallic sulphur, chlorine, nitrogen, oxygen etc. are removed;

[0088] The refined oil obtained after the impurity removal reaction enters the gas-liquid separation tank through a pipeline to separate excess hydrogen and refined oil. The hydrogen is recycled back to the circulating hydrogen compressor 8, and the refined oil flows into the distillation tower 9 through a pipeline;

[0089] S4, the refined oil and refined gas are distilled and separated at 350 ° C in the distillation tower 9, and the dry gas and liquefied gas are extracted from the top of the distillation tower 9; the light cracking oil with a final boiling point of less than 350 ° C flows out of the distillation port of the distillation tower 9; the saturated liquefied gas and oil products with a final boiling point of less than 350 ° C flowing out of the top of the tower are high-quality steam cracking raw materials, which are suitable for most commercial steam cracking furnaces;

[0090] The oil with a fraction greater than 350°C is extracted from the bottom of the fractionating tower. The refined oil with a fraction greater than 350°C is hydrogenated tail oil, which has a chemical composition of saturated alkanes and has good ethylene cracking performance. It is a high-quality ethylene cracking material and can be used as a feedstock for ethylene cracking furnaces with heavy feedstock acceptance capacity.

[0091] The hydrogenation catalyst used in the hydrogenation reaction of S2 and S3 is a composite molecular sieve-supported Ni-Mo series catalyst, the molecular sieve uses hydrogen-type all-silicon MCM-41 and / or HY type molecular sieve, and the molar ratio of Ni to Mo in the catalyst is 3.5:17;

[0092] The silicon content of the gas-liquid phase materials in the reaction effluent is less than 0.5 μg / g, the chlorine content is less than 0.3 μg / g, and the metal content is less than 1 μg / g.

[0093] Example 5 A method for thermal cracking and hydrogenation refining of waste plastics

[0094] First, the circulating hydrogen compressor 8 is turned on, so that the hydrogen begins to circulate along the hydrogen running route B;

[0095] The method for hydrogen pyrolysis and hydrogenation refining of waste plastics involved in the present invention specifically comprises the following steps:

[0096] S1, under hydrogen environment, the mixed waste plastic high-pressure melt is introduced into the hydrogen thermal cracking reactor along the material movement route A, and is subjected to thermal cracking reaction with hydrogen at a reactivity of 480°C and an internal pressure of 1.9MPa to generate waste plastic cracking oil and gas, which is then flowed into the gas-liquid separator 7 for gas-liquid separation to obtain waste plastic cracking gas and waste plastic cracking oil respectively;

[0097] S2, the waste plastic cracking gas enters the gas phase slurry bed hydrogenation reactor 11 along the pipeline, and undergoes hydrogenation reaction under the conditions of reaction temperature of 200° C. and pressure of 2 MPa, wherein hydrogen is 30% in excess of the total amount of the mixed olefin components. The unreacted slurry is re-introduced into the gas phase slurry bed hydrogenation reactor 11 through the slurry circulation pump 12 for continuous hydrogenation reaction. The gas phase hydrogenated saturated gas obtained enters the gas phase fixed bed dechlorination reactor through the pipeline, and undergoes dechlorination reaction under the conditions of 300° C. and 1.6 MPa. The obtained refined gas is introduced into the distillation tower 9 for rectification;

[0098] S3, under the protection of circulating hydrogen, the waste plastics pyrolysis oil is earlier through booster pump 2, and is heated through heat exchanger and process furnace 3 with circulating hydrogen again, the mixed hydrogen material after the heating is 270 ℃ at temperature of reaction through pre-hydrogenation protection reactor 4, refining reactor 5 and dechlorination reactor 6 successively, and pressure is under the condition of 6.3MPa, carry out removing assorted reaction, remove the metallic impurities existing in the plastics pyrolysis oil, as: sodium, calcium and semi-metallic silicon, arsenic and non-metallic sulphur, chlorine, nitrogen, oxygen etc. are removed;

[0099] The refined oil obtained after the impurity removal reaction enters the gas-liquid separation tank through a pipeline to separate excess hydrogen and refined oil. The hydrogen is recycled back to the circulating hydrogen compressor 8, and the refined oil flows into the distillation tower 9 through a pipeline;

[0100] S4, the refined oil and refined gas are distilled and separated at 350 ° C in the distillation tower 9, and the dry gas and liquefied gas are extracted from the top of the distillation tower 9; the light cracking oil with a final boiling point of less than 350 ° C flows out of the distillation port of the distillation tower 9; the saturated liquefied gas and oil products with a final boiling point of less than 350 ° C flowing out of the top of the tower are high-quality steam cracking raw materials, which are suitable for most commercial steam cracking furnaces;

[0101] The oil with a fraction greater than 350°C is extracted from the bottom of the fractionating tower. The refined oil with a fraction greater than 350°C is hydrogenated tail oil, which has a chemical composition of saturated alkanes and has good ethylene cracking performance. It is a high-quality ethylene cracking material and can be used as a feedstock for ethylene cracking furnaces with heavy feedstock acceptance capacity.

[0102] The hydrogenation catalyst used in the hydrogenation reaction of S2 and S3 is a composite molecular sieve-supported Ni-Mo series catalyst, the molecular sieve uses hydrogen-type all-silicon MCM-41 and / or HY type molecular sieve, and the molar ratio of Ni to Mo in the catalyst is 2.3:11;

[0103] The silicon content of the gas-liquid phase materials in the reaction effluent is less than 0.5 μg / g, the chlorine content is less than 0.3 μg / g, and the metal content is less than 1 μg / g. The present invention is further described below with reference to the examples, but the present invention is not limited thereto.

[0104] The dechlorination catalysts involved in Examples 1 to 5 are supported by aluminum oxide, butterfly-shaped, with an equivalent diameter of 1.6 mm, and composed of: sodium carbonate 10 wt.%, magnesium oxide 3.5 wt.%, and calcium content 8.0 wt.%.

[0105] In the examples, the silicon content in the hydrocarbon material was determined using the "Determination of Aluminum, Silicon, Vanadium, Nickel, Iron, Sodium, Calcium, Zinc, and Phosphorus in Residual Fuel Oil - Inductively Coupled Plasma Optical Emission Spectrometry" (IP501-05); the chlorine content in the liquid material was determined using the "Microcoulometric Chlorine Analysis" (ASTM D5808-18). The instrument used was a microcoulometric analyzer, and the sample was a liquid material. The sulfur content was determined using the "Ultraviolet Fluorescence Method" (ASTM D5453); the nitrogen content was determined using the "Standard Test Method for Trace Nitrogen in Liquid Petroleum Hydrocarbons" (ASTM D4629); the total hydrogen content was determined using the "Standard Test Method for Instrumental Determination of Carbon, Hydrogen, and Nitrogen in Petroleum Products and Lubricants" (ASTM D5291); and the group composition was determined using the "Organic Analysis of Distillates by Comprehensive Two-Dimensional Gas Chromatography with Flame Ionization Detection" (UOP990).

[0106] The waste plastic pyrolysis oil prepared from the waste plastic used as raw material in the embodiment contains 401.2 μg / g of sulfur, 86.6 wt.% of carbon, 13 wt.% of hydrogen, 0.28% of oxygen, 563 μg / g of nitrogen, 1503 μg / g of silicon, 4532 μg / g of chlorine, and 620 μg / g of metal content. Its distillation range is 50°C to 550°C, and the group composition contains 48.1 wt.% of paraffins, 41.3 wt.% of cycloalkanes / alkenes / cycloalkenes, and 10.6 wt.% of aromatics and hydrocarbon heteroatom derivatives.

[0107] The product types, yields, and waste plastic recovery rates of the waste plastic crude pyrolysis oil hydrogenation system provided in Examples 1 to 5 are shown in Tables 1 and 2.

[0108] Table 1: Types of oil and gas products from waste plastic pyrolysis and refining

[0109]

[0110] Table 2: Component yield and recovery rate of hydrocarbons from waste plastics

[0111]

[0112] It should be noted that the above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art may still modify the technical solutions described in the above embodiments or replace some of the technical features therein with equivalents. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present invention shall be included within the scope of protection of the present invention.

Claims

1. A method for hydrogen pyrolysis and hydrogenation refining of waste plastics, characterized in that: The method for hydrogen pyrolysis and hydrogenation refining of waste plastics specifically comprises the following steps: S1. In a hydrogen environment, waste plastics enter a hydrogen thermal cracking reactor to undergo a thermal cracking reaction to generate waste plastic cracking oil and gas, which is then flowed into a gas-liquid separation tank for gas-liquid separation to obtain waste plastic cracking gas and waste plastic cracking oil, respectively; the reaction temperature in the waste plastic hydrogen thermal cracking reactor in S1 is 350-550° C., and the pressure in the reactor is 1-2 MPa; S2. In a hydrogen environment, the waste plastic cracking gas passes through a gas phase slurry bed hydrogenation reactor and a gas phase fixed bed dechlorination reactor in sequence, and undergoes olefin saturation, denitrification, desulfurization and dechlorination reactions under the action of a hydrogenation catalyst and a dechlorination agent to obtain a refined gas; the obtained refined gas is introduced into a distillation tower (9) for distillation; The reaction temperature in the gas phase slurry bed hydrogenation reactor in S2 is 150°C to 250°C, and the pressure in the reactor is 1MPa to 2MPa; the reaction temperature of the dechlorination reaction in S2 is 150°C to 250°C, and the pressure is 1MPa to 2MPa; S3, under a hydrogen environment, the waste plastic pyrolysis oil is sequentially passed through a pre-hydrogenation reactor, a refining reactor and a dechlorination reactor under the action of a hydrogenation catalyst and a dechlorinating agent to carry out diene saturation, demetallization, desiliconization, denitrogenation, olefin saturation and dechlorination reactions to obtain refined oil; the obtained refined oil is introduced into a distillation tower (9) for distillation; in S3, the reaction temperature is 200°C to 300°C and the pressure is 4MPa to 8MPa; S4, the refined oil and refined gas are distilled in a distillation tower (9) to obtain saturated dry gas, saturated liquefied gas, light oil and hydrogenated tail oil; The hydrogenation catalyst in S2 and S3 is a composite molecular sieve supported Ni-Mo series catalyst, the molecular sieve uses hydrogen-type all-silicon MCM-41 and / or HY type molecular sieve, and the molar ratio of Ni to Mo in the catalyst is 1.5:2; The dechlorinating agent described in S2 and S3 has a carrier of aluminum oxide in a butterfly shape with an equivalent diameter of 1.6 mm and a composition including: 10 wt. % of sodium carbonate, 3.5 wt. % of magnesium oxide, and 8.0 wt. % of calcium.

2. The method for hydrogen pyrolysis and hydrogenation refining of waste plastics according to claim 1, characterized in that: The waste plastic is at least one of waste plastics in fresh domestic waste, waste plastics in industrial and agricultural production, and waste plastics in aged waste, and the type of the waste plastic is at least one selected from PE, PP, PS, and PVC.

Citation Information

Patent Citations

  • Method for producing fine-quality diesel oil blending component by using waste plastic pyrolysis oil

    CN101724426B

  • Method for producing gasoline and diesel by utilizing plastic oil

    CN102226103A

  • Method and device for preparing clean diesel oil through plastic-converted oil hydrogenation process

    CN102942951A

  • Method for producing clean fuel oil by using waste plastic and high aromatic component

    CN104611060A

  • Method for producing high-quality gasoline / diesel from chlorine-containing plastic oil