A lithium recovery method based on multivalent ion salt-assisted ultrasonic stripping
By using multivalent ion salt-assisted ultrasonic stripping technology in lithium-ion battery recycling, the problem of low lithium extraction efficiency in lithium-ion batteries is solved, and efficient and low-cost lithium recycling and reuse are achieved.
Patent Information
- Application Number
- CN202311864373.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-28
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-12-28
AI Technical Summary
Existing lithium-ion battery recycling methods have low lithium extraction efficiency and low leaching volume, resulting in long-term and high-cost problems.
The multivalent ion salt-assisted ultrasonic stripping method is used to add multivalent ion salts and aromatic hydrocarbon compounds to the lithium extraction reagent, and use ultrasonic technology to accelerate the leaching of lithium, destroy the graphite layer structure, and improve the migration rate and extraction efficiency of lithium.
It significantly shortens the delithiation time of lithium, improves the efficiency of lithium extraction, reduces energy consumption and costs, and achieves efficient recovery and reuse of lithium.
Smart Images

Figure CN117802323B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of waste battery recycling, and more specifically, relates to a lithium recovery method based on multivalent ion salt-assisted ultrasonic stripping. Background Art
[0002] Lithium-ion battery is a secondary battery that mainly relies on the movement of lithium ions between the positive and negative electrodes to work. It is mainly composed of positive electrode materials, negative electrode materials and electrolytes. Lithium-ion batteries are widely used in modern digital products such as mobile phones and laptops. At the same time, with the rapid development of the new energy vehicle industry, the output of lithium-ion batteries has increased rapidly, and a large number of waste lithium-ion batteries will inevitably be generated. Waste lithium-ion batteries contain a large amount of lithium. If the efficient circulation of lithium metal can be achieved, it can not only avoid environmental pollution, but also greatly alleviate the dilemma of my country's shortage of lithium resources.
[0003] In the prior art, CN113061726B discloses a method for safely and efficiently recycling lithium from waste batteries, which is to obtain a lithium-rich solution by directly immersing the negative electrode material in an organic reagent of polycyclic aromatic hydrocarbons. On the one hand, there is a solid-liquid interface between the negative electrode material and the organic reagent, and the reaction rate is slow; on the other hand, graphite has a stable layered structure, and the active lithium embedded in the graphite layers is difficult to react quickly with polycyclic aromatic hydrocarbons. The combined effect of the two leads to low lithium extraction efficiency and leaching amount, which faces the risk of long time and high cost in large-scale applications. Summary of the invention
[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a lithium recovery method based on multivalent ion salt-assisted ultrasonic stripping, aiming to solve the problems of low extraction efficiency and leaching amount of the existing lithium recovery methods.
[0005] To achieve the above object, the present invention provides a lithium recovery method based on multivalent ion salt-assisted ultrasonic stripping, which comprises the following steps:
[0006] S1 uses a lithium extraction reagent to leach the negative electrode material of the waste lithium-ion battery to obtain a solid-liquid mixture, and simultaneously assists ultrasonic stripping to accelerate the leaching of lithium, wherein the lithium extraction reagent is an organic solvent in which an aromatic hydrocarbon compound and a multivalent ion salt are dissolved;
[0007] S2 separates the solid-liquid mixture obtained in step S1 to obtain a lithium-rich solution, thereby realizing efficient recovery of lithium from waste lithium-ion batteries.
[0008] As further preferred, in step S1, during leaching, the mass ratio of the active substance in the negative electrode material to the lithium extraction reagent is 1:1 to 1:5.
[0009] As further preferred, the molar concentration of the aromatic hydrocarbon compound in the lithium extraction reagent is 0.2 mol / L to 3 mol / L, and the mass fraction of the multivalent ion salt is 1% to 5%.
[0010] As further preferred, the aromatic hydrocarbon compound has 6 to 30 carbon atoms and contains at least one benzene ring.
[0011] As a further preference, the aromatic hydrocarbon compound is one or more of benzene, naphthalene, phenanthrene, anthracene, tetracene, pyrene and perylene, and the aromatic hydrocarbon compound includes at least one substituent, and the substituent is an alkyl group, a hydroxyl group, a nitro group, a halogen atom, an amino group, a carboxyl group, an aldehyde group, a carbonyl group, a sulfonic acid group, a disulfide bond, an ester bond or an ether bond.
[0012] As further preferred, the multivalent ion salt is one or more of bistrifluoromethanesulfonyl imide zinc, bistrifluoromethanesulfonyl imide magnesium, bistrifluoromethanesulfonyl imide aluminum and bistrifluoromethanesulfonyl imide calcium.
[0013] As further preferred, the organic solvent is one or more of ethers, esters and aromatics, the ethers include one or more of tetrahydrofuran, ethylene glycol dimethyl ether, 1,3-dioxolane, diethanol dimethyl ether, triethanol dimethyl ether and tetraethanol dimethyl ether; the esters are one or more of ethylene carbonate, propylene carbonate, diethyl carbonate and vinylene carbonate; the aromatics are benzene and / or toluene.
[0014] As further preferred, in step S1, the ultrasonic power is 300W to 3000W, the ultrasonic time is 10min to 10h, and the leaching temperature is -10°C to 100°C.
[0015] As a further preference, the lithium recovery method based on multivalent ion salt-assisted ultrasonic stripping also includes step S3, specifically: soaking the material to be treated with the lithium-rich solution, thereby subjecting the material to be treated to physical and chemical treatment to achieve lithium recycling.
[0016] As a further preference, the material to be treated is a positive electrode of a lithium-ion battery, the positive electrode of the lithium-ion battery is mixed with a lithium extraction reagent, subjected to a hydrothermal reaction, and then dried and washed to obtain a pre-treated positive electrode.
[0017] In general, the above technical solution conceived by the present invention has the following beneficial effects compared with the prior art:
[0018] 1. The present invention adds a multivalent ion salt during the leaching process and combines it with ultrasound assistance. The multivalent ion salt with a larger ion radius can be embedded in the graphite interlayer under ultrasound conditions, thereby accelerating the destruction of the layered structure of the graphite, exposing the active lithium, and making it easier to react with aromatic compounds, thereby optimizing the migration rate of lithium ions and the extraction speed of lithium insertion, greatly shortening the lithium removal time and improving the lithium removal efficiency;
[0019] 2. In particular, the present invention finely controls the content of the multivalent ion salt, which can avoid excessive consumption of lithium extraction reagents when the content of multivalent cations in the solvent is too high. On the other hand, the multivalent cations combined with the aromatic compounds may also cause heteroatom doping of the positive electrode material in the subsequent lithiated positive electrode material. However, since the aromatic compounds combined with lithium in the solution account for the vast majority and have an advantage in kinetics, the above-mentioned effects can be basically ignored.
[0020] 3. At the same time, the present invention can achieve the extraction of active lithium in a shorter time by optimizing the type and content of the aromatic hydrocarbon organic solvent, maximize the role of the lithium extraction reagent, avoid the waste of lithium extraction reagents, the use of a large amount of multivalent ion salts and a longer production time;
[0021] 4. In addition, the present invention can complete lithium extraction at lower energy consumption and cost by optimizing the leaching conditions;
[0022] 5. The present invention also proposes to soak the material to be treated in a lithium-rich solution, thereby enabling rapid and convenient recycling of the recovered lithium. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a lithium recovery flow chart based on multivalent ion salt-assisted ultrasonic stripping provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0025] like Figure 1 As shown, the present invention provides a lithium recovery method based on multivalent ion salt-assisted ultrasonic stripping, the method comprising the following steps:
[0026] S1 uses a lithium extraction reagent to leach the negative electrode of the waste lithium-ion battery to obtain a solid-liquid mixture, and assists ultrasonic stripping to accelerate the leaching of lithium. The lithium extraction reagent is an organic solvent dissolved with aromatic compounds and multivalent ion salts. Because multivalent ions have a large ion radius, they will be embedded in the graphite interlayer under ultrasonic conditions, thereby accelerating the destruction of the layered structure of graphite, thereby stripping the layered graphite, exposing the active lithium, promoting the reaction of active lithium with aromatic compounds, thereby shortening the lithium extraction time and improving the lithium extraction efficiency;
[0027] S2 separates the solid-liquid mixture obtained in step S1 to obtain a lithium-rich solution, thereby realizing efficient recovery of lithium from waste lithium-ion batteries;
[0028] S3 utilizes a lithium-rich solution to soak the material to be processed, thereby subjecting the material to be processed to physical and chemical treatment to achieve lithium recycling.
[0029] Furthermore, in a safe environment with a relative humidity of less than 20% (preferably less than 10%), the waste lithium-ion batteries are fully charged and then disassembled to separate the negative electrode materials and the positive electrode materials. The negative electrode materials are selected from lithium metal negative electrodes, including carbon-based active substances (selected from one or more of natural graphite, artificial graphite, soft carbon, hard carbon, and mesophase carbon microspheres), silicon-based active substances (silicon-based active substances are selected from one or more of silicon element, silicon alloy, and silicon oxide), and the positive electrode materials are selected from lithium iron phosphate in different lithium-containing states, layered ternary materials, lithium manganese oxide, lithium cobalt oxide, lithium-rich manganese materials, etc.
[0030] Further, in step S1, the mass ratio of the active substance in the negative electrode material to the lithium extraction reagent during leaching is 1:1 to 1:5, wherein the mass of the active substance in the negative electrode material is the total mass of the negative electrode material minus the mass of the copper foil, the binder and the conductive agent.
[0031] Within a certain range, the extraction degree and rate of active lithium are related to the amount of lithium extraction reagent added. When the amount of lithium extraction reagent added is insufficient, some lithium in the active substance cannot be combined with aromatic hydrocarbons, and the active lithium cannot be completely extracted, resulting in a low degree of active lithium extraction. On the contrary, when the lithium extraction reagent is much higher than the active substance, the lithium extraction speed and degree will no longer increase significantly, which will cause a waste of lithium extraction reagents and is not conducive to large-scale production. Therefore, the molar concentration of aromatic compounds in the lithium extraction reagent is 0.2mol / L~3mol / L.
[0032] Considering that the multivalent ion salt plays a role in exfoliating the graphite layer and is usually expensive. When the amount of multivalent ion salt added is too little, the graphite structure cannot be completely destroyed, and the time required for lithium extraction will be correspondingly extended. If too much multivalent ion salt is added, the cost will increase significantly. In addition, the solubility of some multivalent ion salts in organic reagents is low, which will also limit the maximum amount of multivalent ion salts added. Therefore, the mass fraction of multivalent ion salts is 1% to 5%. More importantly, the present invention can avoid the situation that when the content of multivalent cations in the solvent is too high, the multivalent cations may combine with aromatic compounds, thereby consuming too much lithium extraction reagents. On the other hand, the multivalent cations combined with aromatic compounds may also cause heteroatom doping of the positive electrode material in the subsequent lithium positive electrode material. However, since the aromatic compounds combined with lithium in the solution account for the vast majority and have an advantage in kinetics, the above-mentioned effects can be basically ignored.
[0033] Furthermore, the aromatic hydrocarbon compound has 6 to 30 carbon atoms and contains at least one benzene ring, which is one or more of benzene, naphthalene, phenanthrene, anthracene, tetracene, pyrene and perylene. The aromatic hydrocarbon compound may also have a substituent, which may be one or more, specifically including an alkyl group, a hydroxyl group, a nitro group, a halogen atom, an amino group, a carboxyl group, an aldehyde group, a carbonyl group, a sulfonic acid group (—SO3H), a disulfide bond (—S—S—), an ester bond (—COO—) or an ether bond (—O—). Among them, groups such as ether bonds can promote complexation with lithium ions, and halogen atoms have greater electron-withdrawing properties, which can increase the polarity of the molecule and promote complexation with lithium ions. These groups can help aromatic hydrocarbon reagents react with lithium ions faster and improve lithium affinity.
[0034] The multivalent ion salt includes one or more of bis(trifluoromethanesulfonyl)imide zinc, bis(trifluoromethanesulfonyl)imide magnesium, bis(trifluoromethanesulfonyl)imide aluminum and bis(trifluoromethanesulfonyl)imide calcium. The multivalent ion salts all contain trifluoromethanesulfonyl hexanes, which is beneficial to reduce the lattice energy of the salt and increase the solubility of the salt in the organic solvent.
[0035] The organic solvent is one or more of ethers, esters and aromatics. The ethers are one or more of tetrahydrofuran, ethylene glycol dimethyl ether, 1,3-dioxolane, diethanol dimethyl ether, triethanol dimethyl ether and tetraethanol dimethyl ether; the esters are one or more of ethylene carbonate, propylene carbonate, diethyl carbonate and vinylene carbonate; the aromatics are benzene and / or toluene.
[0036] Furthermore, if the ultrasonic power is too low, the graphite stripping process is slow, and a longer ultrasonic time is often required to achieve the same degree of stripping, thereby prolonging the time for lithium extraction. Too high ultrasonic power will increase energy consumption, which is not conducive to cost reduction. Ultrasonic time is the lithium extraction time. To a certain extent, extending the ultrasonic time will increase the degree of active lithium extraction, but when the degree of lithium extraction reaches the limit, extending the time will not bring further positive effects. Too short ultrasonic time will cause the lithium extraction reaction to not have enough time to fully occur. The lithium extraction reaction involves a thermodynamic process. A higher temperature will promote the forward reaction, but too high a temperature will cause solvent volatilization, potential side reactions and other problems. The reaction is slow when the temperature is too low, and some solvents may solidify and fail to act. Therefore, in step S2, the ultrasonic power is 300W~3000W, the ultrasonic time is 10min~10h, and the leaching temperature is -10℃~100℃.
[0037] Furthermore, the lithium-rich solution can be applied to the pre-treatment of lithium-ion battery positive electrodes, that is, the material to be treated is a lithium-ion battery positive electrode, and the pre-treatment method includes but is not limited to immersing in the lithium-rich solution, spraying the lithium-rich solution on the surface of the lithium-ion battery positive electrode material, mixing the lithium-ion battery positive electrode material with the lithium-rich solution and then performing a hydrothermal reaction, and then drying and washing to obtain a pre-treated positive electrode.
[0038] The technical solution provided by the present invention is further described below based on specific embodiments.
[0039] Example 1
[0040] (a) dismantling the waste lithium-ion battery in a dry room with a relative humidity of 5%, taking out the dismantled negative electrode sheet and positive electrode sheet, and cutting them into suitable sizes; then preparing a lithium extraction reagent, dissolving 1 mol of biphenyl reagent in 1 L of diethylene glycol dimethyl ether, and then adding 2% by mass of bis(trifluoromethanesulfonyl)imide zinc;
[0041] (b) immersing the negative electrode material in a lithium extraction reagent, wherein the mass ratio of the active material in the negative electrode material to the lithium extraction reagent is 1:2, reacting for 30 minutes at an ultrasonic power of 1000 W and a temperature of 40° C., and then filtering and washing to obtain a lithium-rich solution;
[0042] (c) Immersing the waste positive electrode material in the above lithium-rich solution, stirring and reacting for 5 hours at a temperature of 50° C. After the reaction is completed, washing with diethylene glycol dimethyl ether and drying to obtain a regenerated positive electrode material.
[0043] Example 2
[0044] (a) dismantling the waste lithium-ion battery in a dry room with a relative humidity of 5%, taking out the dismantled negative electrode sheet and positive electrode sheet, and cutting them into suitable sizes; then preparing a lithium extraction reagent, dissolving 3 mol of naphthalene reagent in 1 L of tetrahydrofuran, and then adding 5% by mass of magnesium bis(trifluoromethanesulfonyl)imide;
[0045] (b) immersing the negative electrode material in a lithium extraction reagent, wherein the mass ratio of the active material in the negative electrode material to the lithium extraction reagent is 1:4, reacting for 40 minutes at an ultrasonic power of 3000 W and a temperature of 80° C., and then filtering and washing to obtain a lithium-rich solution;
[0046] (c) Immersing the waste positive electrode material in the above lithium-rich solution, stirring and reacting for 5 hours at a temperature of 50° C. After the reaction is completed, washing with diethylene glycol dimethyl ether and drying to obtain a regenerated positive electrode material.
[0047] Example 3
[0048] (a) dismantling the waste lithium-ion battery in a dry room with a relative humidity of 5%, taking out the dismantled negative electrode sheet and positive electrode sheet, and cutting them into suitable sizes; then preparing a lithium extraction reagent, dissolving 0.2 mol of phenanthrene reagent in 1 L of 1,3-dioxolane, and then adding 1% by mass of bis(trifluoromethanesulfonyl)imide aluminum;
[0049] (b) immersing the negative electrode material in a lithium extraction reagent, wherein the mass ratio of the active material in the negative electrode material to the lithium extraction reagent is 1:1, reacting for 2 h at an ultrasonic power of 300 W and a temperature of -10°C, and then filtering and washing to obtain a lithium-rich solution;
[0050] (c) Immersing the waste positive electrode material in the above lithium-rich solution, stirring and reacting for 5 hours at a temperature of 50° C. After the reaction is completed, washing with diethylene glycol dimethyl ether and drying to obtain a regenerated positive electrode material.
[0051] Example 4
[0052] (a) dismantling the waste lithium-ion battery in a dry room with a relative humidity of 5%, taking out the dismantled negative electrode sheet and positive electrode sheet, and cutting them into suitable sizes; then preparing a lithium extraction reagent, dissolving 2 mol of tetracene reagent in 1 L of triethanol dimethyl ether, and then adding 3% by mass of calcium bis(trifluoromethanesulfonyl)imide;
[0053] (b) immersing the negative electrode material in a lithium extraction reagent, wherein the mass ratio of the active material in the negative electrode material to the lithium extraction reagent is 1:3, reacting for 10 h at an ultrasonic power of 1500 W and a temperature of 30° C., and then filtering and washing to obtain a lithium-rich solution;
[0054] (c) Immersing the waste positive electrode material in the above lithium-rich solution, stirring and reacting for 5 hours at a temperature of 50° C. After the reaction is completed, washing with diethylene glycol dimethyl ether and drying to obtain a regenerated positive electrode material.
[0055] Example 5
[0056] (a) dismantling the waste lithium-ion battery in a dry room with a relative humidity of 5%, taking out the dismantled negative electrode sheet and positive electrode sheet, and cutting them into suitable sizes; then preparing a lithium extraction reagent, dissolving 0.2 mol of 2-methylbiphenyl reagent in 1 L of vinylene carbonate, and then adding 1% by mass of calcium bis(trifluoromethanesulfonyl)imide;
[0057] (b) immersing the negative electrode material in a lithium extraction reagent, wherein the mass ratio of the active material in the negative electrode material to the lithium extraction reagent is 1:5, reacting for 10 min at an ultrasonic power of 300 W and a temperature of 100° C., and then filtering and washing to obtain a lithium-rich solution;
[0058] (c) Immersing the waste positive electrode material in the above lithium-rich solution, stirring and reacting for 5 hours at a temperature of 50° C. After the reaction is completed, washing with diethylene glycol dimethyl ether and drying to obtain a regenerated positive electrode material.
[0059] Comparative Example 1
[0060] The same as Example 1, except that no multivalent ions were introduced into the lithium extraction reagent, no auxiliary ultrasound was introduced, and the leaching time was maintained at 30 min.
[0061] Comparative Example 2
[0062] The same as Example 1, except that no multivalent ions were introduced into the lithium extraction reagent, but auxiliary ultrasound was introduced and the leaching time was maintained at 30 min.
[0063] Comparative Example 3
[0064] As in Example 1, multivalent ions were introduced into the lithium extraction reagent, but auxiliary ultrasound was not introduced, and the leaching time was maintained at 30 min.
[0065] Some reaction conditions and leaching efficiencies of Examples 1-5 and Comparative Examples 1-3 are shown in Table 1. It can be seen that the method of combining multivalent ions and ultrasound was applied in Examples 1-5, and the extraction efficiency reached a high level in a short time. In Comparative Example 1, ultrasound and multivalent ions were not applied, and the lithium extraction efficiency was only 76% in half an hour. Ultrasound or multivalent ions were applied in Comparative Examples 2 and 3, respectively, and the lithium extraction efficiency was slightly improved, but it still could not exceed 90% in a short time. In Examples 1-5, multivalent ions and ultrasound were combined, and the lithium extraction efficiency was able to exceed 90% in a short time, indicating the effectiveness of the method provided by the present invention.
[0066] Table 1 Partial reaction conditions and leaching efficiency of Examples 1-5 and Comparative Examples 1-3
[0067]
[0068]
[0069] The regenerated positive electrode materials obtained in Examples 1-5 and Comparative Examples 1-3 were respectively combined with graphite to form full batteries, and the waste lithium iron phosphate was reassembled into a full battery as Comparative Example 4, and the performance was tested. The data is shown in Figure 2. It can be seen that the first cycle charging capacity of the lithium iron phosphate positive electrode material after regeneration in Examples 1-5 can basically be restored to the level of the theoretical capacity (172 mAhg -1 ), some results are higher than this value, which may be caused by excessive lithium insertion or slight errors during the regeneration process. In contrast, although the performance of the waste lithium iron phosphate can be restored to a certain extent in Comparative Examples 1-3, the degree of recovery is not as good as in the embodiment. There is a certain gap in the cycle performance and the first-cycle efficiency, which may be due to the higher lithium content in the lithium-rich solution of the embodiment, which further reflects the high efficiency of the method. Comparative Example 4 is a full battery reassembled from waste lithium iron phosphate. It can be seen that its performance is poor and it is difficult to continue to meet the use requirements.
[0070] Table 2 Performance data of the full battery composed of regenerated positive electrode materials and graphite
[0071]
[0072] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A lithium recovery method based on multivalent ion salt-assisted ultrasonic stripping, characterized in that: The method comprises the following steps: S1 uses a lithium extraction reagent to leach the negative electrode material of the waste lithium-ion battery to obtain a solid-liquid mixture, and assists ultrasonic stripping to accelerate the leaching of lithium. The lithium extraction reagent is an organic solvent dissolved with aromatic hydrocarbon compounds and multivalent ion salts. The multivalent ion salts all contain trifluoromethanesulfonyl groups, which are beneficial to reducing the lattice energy of the salt and increasing the solubility of the salt in the organic solvent; S2 separates the solid-liquid mixture obtained in step S1 to obtain a lithium-rich solution, thereby realizing efficient recovery of lithium from waste lithium-ion batteries.
2. The lithium recovery method based on multivalent ion salt-assisted ultrasonic stripping according to claim 1, characterized in that: In step S1, during leaching, the mass ratio of the active substance in the negative electrode material to the lithium extraction reagent is 1:1 to 1:
5.
3. The lithium recovery method based on multivalent ion salt-assisted ultrasonic stripping according to claim 1, characterized in that: The molar concentration of the aromatic hydrocarbon compound in the lithium extraction reagent is 0.2 mol / L to 3 mol / L, and the mass fraction of the multivalent ion salt is 1% to 5%.
4. The lithium recovery method based on multivalent ion salt-assisted ultrasonic stripping according to claim 1, characterized in that: The aromatic hydrocarbon compound has 6 to 30 carbon atoms and contains at least one benzene ring.
5. The lithium recovery method based on multivalent ion salt-assisted ultrasonic stripping according to claim 1, characterized in that: The aromatic hydrocarbon compound is one or more of benzene, naphthalene, phenanthrene, anthracene, tetracene, pyrene and perylene, and the aromatic hydrocarbon compound includes at least one substituent, and the substituent is an alkyl group, a hydroxyl group, a nitro group, a halogen atom, an amino group, a carboxyl group, an aldehyde group, a carbonyl group, a sulfonic acid group, a disulfide bond, an ester bond or an ether bond.
6. The lithium recovery method based on multivalent ion salt-assisted ultrasonic stripping according to claim 1, characterized in that: The multivalent ion salt is one or more of bis(trifluoromethanesulfonyl)imide zinc, bis(trifluoromethanesulfonyl)imide magnesium, bis(trifluoromethanesulfonyl)imide aluminum and bis(trifluoromethanesulfonyl)imide calcium.
7. The lithium recovery method based on multivalent ion salt-assisted ultrasonic stripping according to claim 1, characterized in that: The organic solvent is one or more of ethers, esters and aromatics, the ethers include one or more of tetrahydrofuran, ethylene glycol dimethyl ether, 1,3-dioxolane, diethanol dimethyl ether, triethanol dimethyl ether and tetraethanol dimethyl ether; the esters are one or more of ethylene carbonate, propylene carbonate, diethyl carbonate and vinylene carbonate; the aromatics are benzene and / or toluene.
8. The lithium recovery method based on multivalent ion salt-assisted ultrasonic stripping according to claim 1, characterized in that: In step S1, the ultrasonic power is 300W to 3000W, the ultrasonic time is 10min to 10h, and the leaching temperature is -10°C to 100°C.
9. The lithium recovery method based on multivalent ion salt-assisted ultrasonic stripping according to any one of claims 1 to 8, characterized in that: The lithium recovery method based on multivalent ion salt-assisted ultrasonic stripping also includes step S3, which specifically comprises: soaking the material to be treated with the lithium-rich solution, thereby lithiation the material to be treated to achieve lithium recycling.
10. The lithium recovery method based on multivalent ion salt-assisted ultrasonic stripping according to claim 9, characterized in that: The material to be processed is a positive electrode of a lithium-ion battery. The positive electrode of the lithium-ion battery is mixed with a lithium extraction reagent, subjected to a hydrothermal reaction, and then dried and washed to obtain a pre-lithiated positive electrode.