A magnesium alloy brazing material and brazing method
By combining Al-Ag-In ternary alloy brazing filler metal and high-temperature graphite fixtures, the problems of high temperature, poor conductivity and hot cracking in magnesium alloy brazing are solved, realizing high-strength, low-temperature magnesium alloy connection, which is suitable for welding large and complex samples.
Patent Information
- Application Number
- CN202410151456.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-02
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-02-02
AI Technical Summary
Existing magnesium alloy brazing technology suffers from problems such as high brazing temperature, poor conductivity of brazing filler metal, presence of volatile elements, low joint strength, and susceptibility to thermal stress cracking, which affect the connection strength and conductivity of magnesium alloy components.
Using Al-Ag-In ternary alloy brazing filler metal, combined with a high-temperature graphite fixture and a vacuum brazing method, the degree of joint reaction is controlled, the welding temperature is reduced, and the joint strength and conductivity are improved, thus avoiding the generation of hot cracks.
It achieves low-pressure, high-strength magnesium alloy joints without flux assistance, reduces welding temperature, improves joint strength and conductivity, reduces hot cracking, and is suitable for welding large and complex samples.
Smart Images

Figure CN117817184B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of brazing technology, specifically relating to a magnesium alloy brazing material and brazing method. Background Technology
[0002] In recent years, with the continuous development of communication interconnection technology, the requirements for microwave components have been increasing, especially in terms of lightweight and low loss. Using magnesium alloy as the waveguide antenna substrate can achieve both lightweighting and good signal transmission performance. However, brazing of the magnesium alloy is unavoidable during the component manufacturing process.
[0003] Because the oxide film on the surface of magnesium alloys is easily formed at brazing temperatures but difficult to remove, it affects the reaction between the brazing filler metal and the magnesium alloy matrix. Furthermore, the reaction products at the joint are mostly brittle phases, leading to a decrease in joint strength. Secondly, high brazing temperatures soften the base material, thus affecting the performance of magnesium alloy devices. Methods for removing the oxide film from magnesium alloys mainly include using active flux, although flux has some effect, it causes significant corrosion to the base material; or modifying the magnesium alloy surface by plating Cu or Ni, but this modification technique combined with flux-based brazing processes suffers from high electroplating costs, cumbersome procedures, and severe pollution.
[0004] Therefore, vacuum contact reactive brazing is the most economical and efficient process. However, the melting points of existing brazing filler metals used for magnesium alloy brazing are generally high and the degree of eutectic reaction is uncontrollable, which can easily cause softening and excessive corrosion of the magnesium alloy matrix. In addition, the poor conductivity of existing filler metals affects the conductivity of magnesium alloy samples. Furthermore, existing filler metals contain volatile elements (such as Zn), which are not suitable for vacuum brazing. At the same time, the microstructure of vacuum brazed joints of some filler metals is mostly brittle phase, which is prone to hot cracking under temperature conditions during use, resulting in the inability to obtain high-performance welds. Summary of the Invention
[0005] To address the shortcomings of existing technologies, the present invention aims to provide a magnesium alloy brazing material and brazing method, solving the problems of high brazing temperature, poor conductivity of brazing filler metal, presence of volatile elements, low joint strength, and susceptibility to thermal stress cracking in existing vacuum contact reactive brazing of magnesium alloys.
[0006] To achieve the above objectives, the present invention provides the following technical solution: On one hand, the present invention provides a magnesium alloy brazing material, comprising, by weight percentage, 70.0~95.0wt% Al, 4.0~26.0wt% Ag, and 1~5.0wt% In.
[0007] Furthermore, in the magnesium alloy brazing material of the present invention, Al can improve the activity of the brazing filler metal, and its content can be 75.0~90 wt%, including but not limited to 75 wt%, 80 wt%, 85 wt%, and 90 wt%; Ag can balance the plasticity and welding temperature of the brazing filler metal, and the content of Ag in the brazing filler metal can be 8.0~23.0 wt%, including but not limited to 8 wt%, 10 wt%, 15 wt%, and 20 wt%; In can balance the plasticity and welding temperature of the brazing filler metal, and the content of In in the brazing filler metal can be 2.0~4.0 wt%, including but not limited to 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, and 4 wt%. Preferably, the purity of Al, Ag and In is ≥99%.
[0008] On the other hand, the present invention also provides a vacuum brazing method for magnesium alloys, comprising the following steps: S1. Prepare a welding intermediate layer using the brazing material provided in the first aspect above; S2. Take the first magnesium alloy to be welded and the second magnesium alloy to be welded, grind the welding surfaces of the two magnesium alloys to be welded and the two surfaces of the welding intermediate layer, then clean and dry them; S3. The welding surface of the first magnesium alloy to be welded is brought into contact with the first surface of the welding intermediate layer, and the welding surface of the second magnesium alloy to be welded is brought into contact with the second surface of the welding intermediate layer to assemble the workpiece to be welded. S4. The workpiece to be welded is clamped using a brazing fixture, and then vacuum brazing is performed on the workpiece to obtain a brazed magnesium alloy.
[0009] Preferably, the preparation method of the welding intermediate layer in step S1 includes: mixing Al and Ag in proportion, melting under inert gas conditions, and after the metal is completely melted, blowing off the oxide layer on the surface of the molten liquid using inert gas, then adding In to the molten liquid and reheating until the metal melts, and then sequentially performing casting, annealing, and roll forming to obtain the welding intermediate layer.
[0010] Preferably, the melting method is electromagnetic induction heating.
[0011] Preferably, the thickness of the welding intermediate layer is 90~130 μm.
[0012] Preferably, in step S4, the vacuum brazing temperature is 390~470℃, the brazing pressure is 0.01~0.05 MPa, the brazing time is 2~30 min, and the vacuum degree is 2×10⁻⁶. -3 ~7×10 -3 Pa.
[0013] The present invention also provides a brazing fixture, comprising a base with a cavity, a height adjustment member, and a pressure block; the height adjustment member and the pressure block are stacked sequentially in the cavity of the base, and the height adjustment member has an opening for accommodating the workpiece to be welded.
[0014] Preferably, the height adjustment component includes a first shim and a second shim arranged in parallel, and a bolt connecting the first shim and the second shim; the first shim and the second shim are coaxial, and the center of the first shim and the second shim are provided with an opening of the same shape and size.
[0015] Preferably, the raw material for forming the brazing fixture is high-temperature graphite block.
[0016] The beneficial effects of this invention are: The Al-Ag-In brazing filler metal provided by this invention for vacuum contact reactive brazing of magnesium alloys can achieve low-pressure, high-strength joints through chemical potential and concentration differences without flux assistance, resulting in a magnesium alloy vacuum brazed joint strength of 57-68 MPa. It can also significantly reduce the welding temperature by utilizing the Mg-Al-Ag-In quaternary eutectic. The introduction of Ag can significantly increase the conductivity, wettability, and fluidity of the brazing filler metal, and in particular, it can weaken the brittle structure of Mg-Al and improve the shear strength of the joint. The introduction of In can significantly reduce the melting point of the brazing filler metal and lower the welding temperature.
[0017] The brazing filler metal provided by this invention, after melting and rolling, has a fine Al-Ag-In eutectic structure that can be uniformly distributed in the filler metal substrate, reducing the generation of large eutectic structures, refining the grains, thereby improving the overall plasticity, toughness and conductivity of the filler metal, and facilitating the manufacture of large-size filler metal sheets to meet the welding needs of large and complex samples.
[0018] The brazing fixture of the present invention uses high-temperature graphite as the material, and the design of the fixture shape can completely wrap the workpiece, which can make the sample heat up evenly. At the same time, since graphite has the characteristic of slow cooling rate, it can effectively reduce the generation of hot cracks in the brazed joint and improve the joint welding rate.
[0019] The brazing fixture of the present invention controls the degree of joint reaction and improves the joint welding quality by adjusting the height of the height adjustment component to ensure the weld thickness during the contact reaction process. Attached Figure Description
[0020] Figure 1 These are microstructure images of the solder alloys prepared in Examples 1-3; Figure 2 This is a schematic diagram of the sandwich structure of the present invention, showing the workpiece to be welded. Figure 3 This is a three-dimensional structural schematic diagram of the welding fixture according to an embodiment of the present invention; Figure 4 This is a cross-sectional view of the welding fixture according to an embodiment of the present invention; In the diagram, 1 is the base; 2 is the height adjustment component; 21 is the first shim; 22 is the second shim; 23 is the bolt; 3 is the pressure block; and 4 is the part to be welded. Figure 5 These are microstructure images of the brazed joints of Example 1 and Comparative Example 2. Detailed Implementation
[0021] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0022] In the following embodiments, the raw materials were smelted using an SPG-06A-I type high-frequency induction heating device, the brazing sheet was hot rolled using an SC-7063 type double-roller sheet press, the brazing was performed using a VBF-1200X-H8 type horizontal vacuum crucible furnace, the alloy microstructure was observed and photographed using a JXA-8230 type electron probe, and the tensile test was performed using a QJ-210A-5000N type mechanical property tensile tester.
[0023] The raw materials Al, Ag and In used in the examples all have a purity of 99.99 wt%, are granular, and have an average size of 2×2×2 mm.
[0024] Example 1 A vacuum brazing method for magnesium alloys includes the following steps: (1) Preparation of welding intermediate layer The brazing filler metal consists of 75 wt% Al, 23 wt% Ag, and 2 wt% In. It is melted using electromagnetic induction heating with an SPG-06A-I type induction heater and a corundum + graphite crucible protected by argon gas. The induction melting furnace is operated through multiple cycles of vacuuming and high-purity argon gas circulation. First, Al and Ag are mixed in the specified proportions and induction melted under high-purity argon conditions. After the metal is completely melted, the oxide layer on the surface of the molten liquid is blown off using high-purity compressed argon gas. In is then added, and the temperature is raised again until the metal melts. The process then involves casting, annealing, and roll forming. The brazing filler metal is formed into a sheet, resulting in a 10mm × 10mm × 0.12mm intermediate welding layer.
[0025] (2) Pretreatment of base material and welding intermediate layer Take two pieces of base material (AZ31 magnesium alloy) with a size of 10mm×10mm×3mm and one welding intermediate layer. Grind the welding surfaces of the two magnesium alloys to be welded and the upper and lower surfaces of the welding intermediate layer to remove the oxide film on the surface. Then place them in anhydrous ethanol for ultrasonic cleaning for 1 minute and blow dry.
[0026] (3) Assemble the parts to be welded Place the first magnesium alloy to be welded with its welding surface facing upwards, and place the intermediate welding layer on top of it. Place the second magnesium alloy to be welded with its welding surface facing downwards on top of the intermediate welding layer. Figure 2 As shown, the components to be welded are assembled into a sandwich structure.
[0027] (4) Vacuum brazing The workpiece to be brazed in step (3) is clamped using a brazing fixture, and then placed in a vacuum crucible furnace for brazing. The brazing temperature is 410℃, the brazing pressure is 0.03MPa, and the vacuum degree is 5×10⁻⁶. -3 Pa, brazing time of 15 min, to obtain brazed magnesium alloy.
[0028] The brazing fixture used in this embodiment is made from high-temperature graphite blocks, such as... Figures 3-4 As shown, it includes a base 1, a height adjustment component 2, and a pressure block 3. The base 1 has a cubic cavity at its center, which is used to fully enclose the sample to ensure uniform heating and cooling.
[0029] The height adjustment component 2 includes a first washer 21 and a second washer 22 arranged in parallel, and a bolt 23 connecting the first washer and the second washer. The first washer 21 and the second washer 22 have openings of the same shape and size at their centers. Specifically, the first washer 21 and the second washer 22 are two square rings of the same shape and size, and threaded holes are provided at the diagonal corners of the upper and lower square rings. The bolt 23 is threadedly connected through the threaded holes between the upper and lower rings. In use, firstly, the distance between the first washer and the second washer is adjusted by turning the bolt 23 according to the preset thickness of the magnesium alloy after welding. Then, the height adjustment component 2 is placed flat in the cavity of the base 1. Next, the sandwich-structured workpiece 4 to be welded is stacked and placed at the center opening of the height adjustment component 2, with the thickness of the workpiece to be welded slightly higher than the height of the height adjustment component 2. Finally, the pressure block 3 is placed on top of the workpiece to be welded to complete the clamping.
[0030] The principle of the brazing fixture of the present invention is as follows: when the assembled workpiece is placed in the vacuum crucible furnace, as the reaction proceeds, the workpiece is continuously pressed down under the action of the pressure block until the pressure block contacts the first shim of the height adjustment component. At this time, the height adjustment component supports the pressure block and prevents it from further applying pressure to the workpiece, which would cause the height of the workpiece to drop, thereby controlling the degree of joint reaction.
[0031] The microstructure of the solder alloy after induction melting in this embodiment is shown in the figure. Figure 1(a) shows that the fine Al-Ag-In eutectic structure can be uniformly distributed in the brazing filler metal substrate after melting and rolling, reducing the formation of large eutectic structures, refining grains, and thus improving the overall plasticity, toughness, and conductivity of the brazing filler metal, facilitating the manufacture of large-size brazing filler metal sheets. The thickness of the intermediate layer was rolled to 120 μm, the peak melting temperature of the brazing filler metal was 566℃, and the tensile strength of the brazing filler metal was 122 MPa. The height of the magnesium alloy after brazing was 6 mm, the average shear strength of the brazed butt joint was 62 MPa, the joint weld rate was 97%, and the joint micromorphology was as follows. Figure 5 As shown in (a), the joint is flat and free of defects such as thermal cracks.
[0032] Example 2 A vacuum brazing method for magnesium alloys is basically the same as that in Example 1, except that the composition of the brazing filler metal in step (1) when preparing the intermediate layer includes 70wt% Al, 26wt% Ag and 4wt% In.
[0033] The microstructure of the solder alloy in this embodiment is as follows: Figure 1 As shown in (b), the brazing filler metal thickness can be rolled to 130 μm, the peak melting temperature of the filler metal is 552 °C, and the tensile strength of the filler metal is 114 MPa. The average shear strength of the brazed butt joint is 67 MPa, and the joint weld rate is 97.3%.
[0034] Example 3 A vacuum brazing method for magnesium alloys is basically the same as that in Example 1, except that the composition of the brazing filler metal in step (1) when preparing the intermediate layer includes 90wt% Al, 8wt% Ag and 2wt% In.
[0035] The microstructure of the solder alloy in this embodiment is as follows: Figure 1 As shown in (c), the brazing filler metal thickness can be rolled to 100 μm, the peak melting temperature of the filler metal is 623℃, and the tensile strength of the filler metal is 112 MPa. The average shear strength of the brazed butt joint is 58 MPa, and the joint weld ratio is 93.5%.
[0036] Example 4 A vacuum brazing method for magnesium alloys is basically the same as that in Example 1, except that the composition of the brazing filler metal in step (1) when preparing the intermediate layer includes 95wt%Al, 4wt%Ag and 1wt%In.
[0037] In this embodiment, the brazing filler metal thickness can be rolled to 90 μm, the peak melting temperature of the filler metal is 652°C, and the tensile strength of the filler metal is 93 MPa. The average shear strength of the brazed butt joint is 57 MPa, and the joint weld rate is 93.4%.
[0038] Example 5 A vacuum brazing method for magnesium alloys is basically the same as that in Example 1, except that the composition of the brazing filler metal in step (1) when preparing the intermediate layer includes 70wt% Al, 25wt% Ag and 5wt% In.
[0039] In this embodiment, the brazing filler metal thickness can be rolled to 130 μm, the peak melting temperature of the filler metal is 550°C, and the tensile strength of the filler metal is 113 MPa. The average shear strength of the brazed butt joint is 68 MPa, and the joint weld rate is 97.4%.
[0040] Comparative Example 1 A vacuum brazing method for magnesium alloys is basically the same as that in Example 1, except that the composition of the brazing filler metal in step (1) when preparing the intermediate layer includes 60wt% Al, 30wt% Ag and 10wt% In.
[0041] The brazing alloy has poor plasticity and cannot be made into brazing sheets, making it unsuitable as a brazing system for brazing magnesium alloys.
[0042] Comparative Example 2 A vacuum brazing method for magnesium alloys is basically the same as that in Example 1, except that a brazing fixture is not used for clamping during the vacuum brazing process in step (4). The microstructure of the joint is as follows. Figure 5 As shown in (b), thermal cracks appeared at the joint interface, the degree of reaction was inconsistent at different locations of the joint, and there was severe overflow. The average shear strength of the joint was 45 MPa, and the joint weld rate was 69%.
[0043] For ease of comparison, the raw material usage of the above embodiments and comparative examples is listed in Table 1.
[0044] Table 1
[0045] As shown in Table 1, the Al-Ag-In ternary alloy brazing filler metal provided by this invention lowers the melting point due to the introduction of Ag and In, and also reduces the melting point of the Mg-Al-Ag-In quaternary alloy system during welding. This allows the welding temperature to be lowered to 390~470℃ during contact reaction welding, ensuring brazing of magnesium alloys at lower temperatures and avoiding overheating of the base material. The filler metal exhibits good plasticity and high toughness, enabling high-strength connections of magnesium alloys without the need for flux.
[0046] Compared with Comparative Example 2, Example 1 is as follows: Figure 5 As shown, the brazing fixture of the present invention can significantly reduce the generation of hot cracks in brazed joints, improve the joint welding rate, accurately control the degree of joint reaction, and improve the joint welding quality.
[0047] In summary, the magnesium alloy brazing material provided by this invention can achieve high-strength welding under low pressure and vacuum rupture without flux assistance, and can significantly reduce the welding temperature, effectively avoiding the problem of overheating and softening during high-temperature brazing of magnesium alloys. The brazing filler metal has good plasticity and high toughness, and can be cut into various sizes to meet the welding requirements of complex samples. At the same time, it has excellent conductivity, which is sufficient to meet the brazing requirements of magnesium alloy workpieces with electrical signal requirements. The brazing fixture used in conjunction can reduce thermal stress cracking of the joint, improve the joint welding rate, and make the degree of joint reaction controllable, making it suitable for large-scale industrial promotion.
[0048] It should be noted that all the above embodiments belong to the same inventive concept, and the descriptions of each embodiment have different focuses. Where the description in a particular embodiment is not detailed, please refer to the description in other embodiments.
[0049] The embodiments described above are merely illustrative of implementation methods of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A vacuum brazing method for magnesium alloys, characterized in that, Includes the following steps: S1. A magnesium alloy brazing material is used to prepare the intermediate welding layer; S2. Take the first magnesium alloy to be welded and the second magnesium alloy to be welded, grind the welding surfaces of the two magnesium alloys to be welded and the two surfaces of the welding intermediate layer, then clean and dry them; S3. The welding surface of the first magnesium alloy to be welded is brought into contact with the first surface of the welding intermediate layer, and the welding surface of the second magnesium alloy to be welded is brought into contact with the second surface of the welding intermediate layer to assemble the workpiece to be welded. S4. The workpiece to be welded is clamped using a brazing fixture, and then vacuum brazed to obtain a brazed magnesium alloy sample; wherein, The magnesium alloy brazing material comprises, by weight percentage: Al 70.0~95.0 wt%, Ag 4.0~26.0 wt%, In 1~5.0 wt%; The brazing fixture includes a base with a cavity, a height adjustment component, and a pressure block; the height adjustment component and the pressure block are stacked sequentially in the cavity of the base, and the height adjustment component has an opening for accommodating the workpiece to be welded; The workpieces to be welded are stacked on top of the central opening of the height adjustment component, and the thickness of the workpieces to be welded is slightly higher than the height of the height adjustment component. The pressure block is placed on top of the workpieces to be welded. The vacuum brazing temperature in step S4 is 390~470℃, the brazing pressure is 0.01~0.05 MPa, the brazing time is 2~30 min, and the vacuum degree is 2×10⁻⁶. -3 ~7×10 -3 Pa.
2. The vacuum brazing method for magnesium alloys according to claim 1, characterized in that, The purity of Al, Ag and In in the raw materials of the magnesium alloy brazing material is ≥99%.
3. The vacuum brazing method for magnesium alloys according to claim 1, characterized in that, The preparation method of the welding intermediate layer in step S1 includes: mixing Al and Ag in proportion, melting under inert gas conditions, and after the metal is completely melted, blowing off the oxide layer on the surface of the molten liquid using inert gas, then adding In to the molten liquid and reheating until the metal melts, and then sequentially casting, annealing, and roll forming to obtain the welding intermediate layer.
4. The vacuum brazing method for magnesium alloys according to claim 3, characterized in that, The smelting method is electromagnetic induction heating.
5. The vacuum brazing method for magnesium alloys according to claim 1, characterized in that, The thickness of the welding intermediate layer is 90~130 μm.
6. The vacuum brazing method for magnesium alloys according to claim 1, characterized in that, The height adjustment component includes a first shim and a second shim arranged in parallel, and a bolt connecting the first shim and the second shim; the first shim and the second shim are coaxial, and the center of the first shim and the second shim are provided with an opening of the same shape and size.
7. The vacuum brazing method for magnesium alloys according to claim 1, characterized in that, The raw material used to form the brazing fixture is high-temperature graphite block.
Citation Information
Patent Citations
Brazing filler metal for magnesium alloy, using method and soldering flux of brazing filler metal
CN115502604A
Magnesium alloy current auxiliary vacuum brazing tool and brazing method
CN116944614A