Ecological concrete and production process thereof

By using the combination of silicon brick powder and peat soil in ecological concrete, the problems of poor moisture storage and high alkalinity of ecological concrete are solved, better moisture replenishment and plant growth environment are achieved, and the prospects for use of ecological concrete are improved.

CN117819922BActive Publication Date: 2024-11-22TONGLU DINGLI BUILDING MATERIALS CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202311812031.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-27
Publication Date
2024-11-22
Estimated Expiration
2043-12-27

AI Technical Summary

Technical Problem

During the preparation process of general ecological concrete on the market, its water storage capacity is poor, making it difficult to replenish vegetation moisture, water loss is rapid, and the internal alkalinity of the concrete is too high, resulting in the inability to meet the normal environmental needs of plant growth.

Method used

In the production process of ecological concrete, the improved moisture storage can be prepared by filling the block base of silicon brick powder with peat soil, combined with cement, limestone, fly ash, aggregate and other materials, and stirring and rolling steps are used to prepare the process of improving moisture storage and Ecological concrete with alkalinity neutralization effect.

Benefits of technology

It effectively improves the moisture storage capacity of ecological concrete, meets the normal environmental needs of plant growth, extends the time for moisture replenishment, and improves the suitability of vegetation growth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117819922B_ABST
    Figure CN117819922B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of preparation of ecological concrete, and specifically to a production process of ecological concrete, and the production steps are as follows: S1, prepare the following raw materials: 10-500 parts of cement, 20-200 parts of limestone, 100-800 parts of fly ash, 200-600 parts of aggregate, 20-100 parts of reinforcing agent, 1-60 parts of water reducer, 1-200 parts of silica brick powder, 20-300 parts of peat soil, 1-50 parts of defoaming agent and 100-2000 parts of water. The present application adds a block base made of silica brick powder to the bottom of the ecological concrete, and peat soil is filled in the silica brick powder, which can effectively lock the moisture, improve the water storage capacity, and supplement the moisture of the vegetation. The alkalinity inside the concrete is neutralized to a certain extent by silica brick powder, so as to better meet the normal environmental requirements of plant growth, so that the ecological concrete can better ensure the regulation of the environment, and bring better prospects for use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ecological concrete preparation, in particular to ecological concrete and its production process. Background Art

[0002] Ecological concrete, referred to as vegetation concrete, is also known as "vegetation concrete", "vegetation concrete", "greening concrete", "ecological anti-filtration vegetation concrete", etc. Its main body uses aggregate of specific particle size as the supporting skeleton, and is wrapped with ecological cementitious materials and aggregates. It has a certain pore structure and strength. Ecological concrete can achieve ecological planting while achieving safety protection. It is a new type of slope protection material that can combine engineering protection and ecological restoration. It can reduce the amount of cement, has dust removal and noise reduction, water permeability and air permeability, water purification and heat storage, and is environmentally friendly or biocompatible. Ecological concrete has a broad and narrow conceptual distinction. The broad definition of ecological concrete is to have certain ecological effects or specific ecological functions. Concrete, compared with traditional concrete, generally has the above functions. In a narrow sense, ecological concrete is, in short, concrete with biocompatibility and ecological effects. The ecological effect can be expressed as the finished concrete can grow organisms and affect organisms. The organisms attached to the concrete have a dependent relationship with the concrete. It specifically refers to concrete, concrete structures and concrete products with good biocompatibility. However, the general ecological concrete on the market has poor water storage capacity during the preparation process, making it difficult to replenish water for vegetation. The water loss is rapid, and the alkalinity inside the concrete is too high, which makes it impossible to meet the normal environmental needs of plant growth. In this regard, we proposed an ecological concrete and its production process. Summary of the invention

[0003] In view of the deficiencies of the prior art, the present invention provides an ecological concrete and a production process thereof to solve the above technical problems.

[0004] To achieve the above object, the present invention provides the following technical solution: a production process of ecological concrete, the production steps are:

[0005] S1. Prepare the following raw materials: 10-500 parts of cement, 20-200 parts of limestone, 100-800 parts of fly ash, 200-600 parts of aggregate, 20-100 parts of reinforcing agent, 1-60 parts of water reducing agent, 1-200 parts of silica brick powder, 20-300 parts of peat soil, 1-50 parts of defoaming agent and 100-2000 parts of water;

[0006] S2, adding water to the silica brick powder and mixing, pouring it into the block-shaped mold, sending it to be fired, and processing the silica brick powder into the shape of the mold;

[0007] S3, adding peat soil into the material prepared in step S2 to fill the middle hole;

[0008] S4, pouring cement, limestone, fly ash and water into a mixing device for mixing and mixing evenly;

[0009] S5. During the stirring process, the reinforcing agent, water reducing agent and defoaming agent are continuously added and mixed and stirred;

[0010] S6. Filling aggregate on top of the material prepared in step S3;

[0011] S7, pouring the concrete mixed in step S5 onto the top of the aggregate for molding, and using a rolling device to continuously roll the upper surface to improve compactness;

[0012] S8. The formed ecological concrete is cured. After the curing is completed, the concrete is removed from the mold to complete the preparation.

[0013] Preferably, in step S2, the shape of the mold is a cube with a hollowed-out middle, and the firing time is 5 hours. In step S3, the middle of the mold is filled and pressed to be compacted. In step S4, the stirring time is 2 hours and the stirring speed is 30 r / min.

[0014] Preferably, in step S5, after stirring in the stirring equipment for 30 minutes, a reinforcing agent is added into the stirring equipment, after stirring in the stirring equipment for 1.5 hours, a water reducing agent is added into the stirring equipment, after stirring in the stirring equipment for 1.8 hours, a defoaming agent is added into the stirring equipment, the aggregate selected in step S6 is crushed stone, the thickness of the aggregate layer is 50 mm, and the curing time in step S8 is 3 days.

[0015] An ecological concrete, which is prepared by the production process of an ecological concrete described in any one of the above items, and the ecological concrete comprises the following materials: 10-500 parts of cement, 20-200 parts of limestone, 100-800 parts of fly ash, 200-600 parts of aggregate, 20-100 parts of reinforcing agent, 1-60 parts of water reducing agent, 1-200 parts of silica brick powder, 20-300 parts of peat soil, 1-50 parts of defoaming agent and 100-2000 parts of water.

[0016] Preferably, 450 parts of cement, 100 parts of limestone, 150 parts of fly ash, 540 parts of aggregate, 80 parts of reinforcing agent, 40 parts of water reducing agent, 150 parts of silica brick powder, 220 parts of peat soil, 25 parts of defoaming agent and 1000 parts of water.

[0017] Preferably, the type of cement is one of silicate cement, aluminate cement and sulphoaluminate cement, and the preparation steps of cement are as follows: prepare cement quartz, limestone and clay; crush the raw materials in the cement plant, grind the large pieces of quartz, limestone and clay into powder respectively, and use a hammer crusher as the equipment; mix the quartz powder, limestone powder and clay powder according to a predetermined ratio to obtain a new material; put the mixture into a rotary kiln, and burn it at a high temperature of 1400-1500°C in the rotary kiln. During the burning period, the quartz and limestone react chemically under high temperature conditions and combine to form cement solids; after the burning is completed, the cement solids are gradually cooled and discharged from the top of the rotary kiln. The discharged cement solids are then crushed, screened and graded to obtain cement products of standard specifications.

[0018] Preferably, the limestone is one of high-calcium limestone, low-calcium limestone and gypsum limestone. The preparation steps of the limestone are to mine the limestone ore by blasting, crush the mined limestone ore, crush the large pieces of limestone into smaller particles, place the particles in a lime kiln for calcining, grind the calcined material to obtain limestone, wherein the ratio of cement to limestone is 4.5:1.

[0019] Preferably, the fly ash is one of bituminous coal fly ash, bituminous coal peat ash and anthracite fly ash. The preparation steps of the fly ash are to select coal suitable for producing fly ash, crush and grind the selected coal to achieve the required fineness, burn the crushed fly coal through a combustion device to generate high-temperature flue gas and ash, and the generated high-temperature flue gas is treated by a dust collector and a desulfurization device to remove dust and harmful gases. The ash generated after combustion is treated with a dust collector to remove dust and is collected in a centralized manner. Aggregates include sand, gravel, crushed stone, slag and concrete. The ratio of fly ash to aggregate is 1.5:5.4.

[0020] Preferably, the enhancer is a silicate enhancer, and the preparation steps of the enhancer are to prepare silicate, cement and gypsum raw materials; according to the prescribed formula ratio, the raw materials are placed in a mixer for mixing and stirring, stirring evenly, adding an appropriate amount of water or other additives, adjusting the consistency of the silicate enhancer, and storing the prepared silicate enhancer in a dry and cool environment to avoid direct sunlight and moisture. The preparation steps of the water reducer are to add various raw materials to a mixing device, ensure that the quality and proportion of the raw materials meet the production requirements, fully stir and mix evenly, filter the mixed ingredients through a filtering device to remove impurities and solid particles therein, dehydrate, grind the filtered and dehydrated ingredients, send the ground raw materials into a reactor, add a certain solvent and catalyst, and synthesize the water reducer through reaction.

[0021] Preferably, the silica brick powder is obtained by crushing silica bricks, the peat soil is sphagnum peat soil, and the preparation step of the defoamer is to react alcohol with sulfuric acid to obtain ether, the reaction needs to be carried out in an acidic environment, and heating is required to promote the reaction, and after the reaction is completed, the ether is extracted from the reaction mixture by distillation;

[0022] Oxidize n-octane to obtain octanal, then reduce octanal to obtain octanol, add sodium sulfate into a mixer, add silicone emulsion thereto, and stir evenly; then add sodium sulfate thereto, stir evenly, add silicone emulsion, stir evenly, add sodium citrate and maleic acid acrylic acid copolymer, continue stirring, add anhydrous ethanol and deionized water after stirring evenly, stir evenly, and then granulate and dry the obtained mixture.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] This application adds a block base made of silica brick powder to the bottom of the ecological concrete, and fills the silica brick powder with peat soil, which can effectively lock in moisture, improve water storage capacity, and supplement moisture for vegetation. The alkalinity inside the concrete is neutralized to a certain extent by the silica brick powder to better meet the normal environmental requirements of plant growth, bringing better usage prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a process diagram of preparing ecological concrete according to the present invention;

[0026] Figure 2 This is an analysis diagram of the overall structure of the ecological concrete of the present invention. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] The present invention provides a technical solution: a production process of ecological concrete, the production steps are:

[0029] S1. Prepare the following raw materials: 10-500 parts of cement, 20-200 parts of limestone, 100-800 parts of fly ash, 200-600 parts of aggregate, 20-100 parts of reinforcing agent, 1-60 parts of water reducing agent, 1-200 parts of silica brick powder, 20-300 parts of peat soil, 1-50 parts of defoaming agent and 100-2000 parts of water;

[0030] S2, adding water to the silica brick powder and mixing, pouring it into the block-shaped mold, sending it to be fired, and processing the silica brick powder into the shape of the mold;

[0031] S3, adding peat soil into the material prepared in step S2 to fill the middle hole;

[0032] S4, pouring cement, limestone, fly ash and water into a mixing device for mixing and mixing evenly;

[0033] S5. During the stirring process, the reinforcing agent, water reducing agent and defoaming agent are continuously added and mixed and stirred;

[0034] S6. Filling aggregate on top of the material prepared in step S3;

[0035] S7, pouring the concrete mixed in step S5 onto the top of the aggregate for molding, and using a rolling device to continuously roll the upper surface to improve compactness;

[0036] S8. The formed ecological concrete is cured. After the curing is completed, the concrete is removed from the mold to complete the preparation.

[0037] Furthermore, in step S2, the shape of the mold is a cube with a hollowed-out middle, and the firing time is 5 hours. In step S3, the middle of the mold is filled and pressed to be compacted. In step S4, the stirring time is 2 hours and the stirring speed is 30 r / min.

[0038] Furthermore, in step S5, after stirring in the stirring equipment for 30 minutes, a reinforcing agent is added into the stirring equipment, after stirring in the stirring equipment for 1.5 hours, a water reducing agent is added into the stirring equipment, after stirring in the stirring equipment for 1.8 hours, a defoaming agent is added into the stirring equipment, the aggregate selected in step S6 is crushed stone, the thickness of the aggregate layer is 50 mm, and the curing time in step S8 is 3 days.

[0039] An ecological concrete is prepared by any of the above items, and the ecological concrete comprises the following materials: 10-500 parts of cement, 20-200 parts of limestone, 100-800 parts of fly ash, 200-600 parts of aggregate, 20-100 parts of reinforcing agent, 1-60 parts of water reducing agent, 1-200 parts of silica brick powder, 20-300 parts of peat soil, 1-50 parts of defoaming agent and 100-2000 parts of water.

[0040] Furthermore, 450 parts of cement, 100 parts of limestone, 150 parts of fly ash, 540 parts of aggregate, 80 parts of reinforcing agent, 40 parts of water reducing agent, 150 parts of silica brick powder, 220 parts of peat soil, 25 parts of defoaming agent and 1000 parts of water.

[0041] Furthermore, the type of cement is one of silicate cement, aluminate cement and sulphoaluminate cement, and the preparation steps of cement are: prepare cement quartz, limestone and clay; the raw materials are crushed in the cement plant, and large pieces of quartz, limestone and clay are ground into powder respectively, and the equipment used is a hammer crusher; the quartz powder, limestone powder and clay powder are mixed according to a predetermined ratio to obtain a new material; the mixture is put into a rotary kiln, and fired at a high temperature of 1400-1500°C in the rotary kiln. During the firing, the quartz and limestone react chemically under high temperature conditions and combine to form cement solids; after the firing is completed, the cement solids are gradually cooled and discharged from the top of the rotary kiln, and the discharged cement solids are crushed, screened and graded to obtain cement products of standard specifications.

[0042] Furthermore, the limestone is one of high-calcium limestone, low-calcium limestone and mud limestone. The preparation steps of the limestone are to mine the limestone ore by blasting, crush the mined limestone ore, crush the large pieces of limestone into smaller particles, place the particles in a lime kiln for calcining, grind the calcined material to obtain limestone, wherein the ratio of cement to limestone is 4.5:1.

[0043] Furthermore, the fly ash is one of bituminous coal fly ash, bituminous coal peat ash and anthracite fly ash. The preparation steps of the fly ash are to select coal suitable for producing fly ash, crush and grind the selected coal to achieve the required fineness, burn the crushed fly coal through combustion equipment to generate high-temperature flue gas and ash, and the generated high-temperature flue gas is treated by a dust collector and a desulfurization equipment to remove dust and harmful gases. The ash generated after combustion is treated with a dust collector for dust removal and centralized collection. Aggregates include sand, gravel, crushed stone, slag and concrete. The ratio of fly ash to aggregate is 1.5:5.4.

[0044] Furthermore, the reinforcing agent is a silicate reinforcing agent, and the preparation steps of the reinforcing agent are to prepare silicate, cement and gypsum raw materials; according to the prescribed formula ratio, the raw materials are put into a mixer for mixing and stirring, stirring evenly, adding an appropriate amount of water or other additives, adjusting the consistency of the silicate reinforcing agent, and storing the prepared silicate reinforcing agent in a dry and cool environment to avoid direct sunlight and moisture. The preparation steps of the water reducing agent are to add various raw materials into a mixing device, ensure that the quality and proportion of the raw materials meet the production requirements, fully stir and mix evenly,

[0045] The mixed ingredients are filtered through a filtering device to remove impurities and solid particles therein, and dehydrated. The filtered and dehydrated ingredients are ground, and the ground raw materials are sent to a reactor, and a certain solvent and catalyst are added to synthesize a water reducer through reaction.

[0046] Furthermore, the silica brick powder is obtained by crushing silica bricks, the peat soil is sphagnum peat soil, and the preparation step of the defoamer is to react alcohol with sulfuric acid to obtain ether, the reaction needs to be carried out in an acidic environment, and heating is required to promote the reaction, and after the reaction is completed, the ether is extracted from the reaction mixture by distillation;

[0047] Oxidize n-octane to obtain octanal, then reduce octanal to obtain octanol, add sodium sulfate into a mixer, add silicone emulsion into the mixer, and stir evenly; then add sodium sulfate into the mixer, stir evenly, add silicone emulsion into the mixer, stir evenly, add sodium citrate and maleic acid acrylic acid copolymer, continue stirring, add anhydrous ethanol and deionized water into the mixer, stir evenly, and granulate and dry the obtained mixture;

[0048] Defoamers have the following advantages: strong defoaming power, small dosage, no effect on the basic properties of the system when added to the foaming system, i.e. no reaction with the defoamed system, small surface tension, good balance with the surface, good heat resistance, good diffusivity and permeability, high positive spreading coefficient, chemical stability, strong oxidation resistance, good gas solubility and permeability, low solubility in foaming solutions, no physiological activity, and high safety;

[0049] Silica brick powder has high fire resistance and thermal stability. As an acidic substance, it can maintain excellent thermal shock resistance and chemical corrosion resistance at high temperatures, so it is an ideal furnace lining material. Secondly, silica brick powder has high strength and good wear resistance, and can withstand the wear and impact of heavy objects. In addition, silica brick powder has good thermal conductivity, which can effectively transfer heat and reduce heat loss. Example

[0050] A production process of ecological concrete, the production steps are:

[0051] S1. Prepare the following raw materials: 450 parts of cement, 100 parts of limestone, 150 parts of fly ash, 540 parts of aggregate, 80 parts of reinforcing agent, 40 parts of water reducing agent, 150 parts of silica brick powder, 220 parts of peat soil, 25 parts of defoaming agent and 1000 parts of water;

[0052] S2, adding water to the silica brick powder and mixing, pouring it into the block-shaped mold, sending it to be fired, and processing the silica brick powder into the shape of the mold;

[0053] S3, adding peat soil into the material prepared in step S2 to fill the middle hole;

[0054] S4, pouring cement, limestone, fly ash and water into a mixing device for mixing and mixing evenly;

[0055] S5. During the stirring process, the reinforcing agent, water reducing agent and defoaming agent are continuously added and mixed and stirred;

[0056] S6. Filling aggregate on top of the material prepared in step S3;

[0057] S7, pouring the concrete mixed in step S5 onto the top of the aggregate for molding, and using a rolling device to continuously roll the upper surface to improve compactness;

[0058] S8. The formed ecological concrete is cured. After the curing is completed, the concrete is removed from the mold to complete the preparation. Example

[0059] A production process of ecological concrete, the production steps are:

[0060] S1. Prepare the following raw materials: 500 parts of cement, 20 parts of limestone, 500 parts of fly ash, 250 parts of aggregate, 50 parts of reinforcing agent, 55 parts of water reducing agent, 10 parts of silica brick powder, 25 parts of peat soil, 50 parts of defoaming agent and 800 parts of water;

[0061] S2, adding water to the silica brick powder and mixing, pouring it into the block-shaped mold, sending it to be fired, and processing the silica brick powder into the shape of the mold;

[0062] S3, adding peat soil into the material prepared in step S2 to fill the middle hole;

[0063] S4, pouring cement, limestone, fly ash and water into a mixing device for mixing and mixing evenly;

[0064] S5. During the stirring process, the reinforcing agent, water reducing agent and defoaming agent are continuously added and mixed and stirred;

[0065] S6. Filling aggregate on top of the material prepared in step S3;

[0066] S7, pouring the concrete mixed in step S5 onto the top of the aggregate for molding, and using a rolling device to continuously roll the upper surface to improve compactness;

[0067] S8. The formed ecological concrete is cured. After the curing is completed, the concrete is removed from the mold to complete the preparation. Example

[0068] A production process of ecological concrete, the production steps are:

[0069] S1. Prepare the following raw materials: 250 parts of cement, 180 parts of limestone, 150 parts of fly ash, 600 parts of aggregate, 100 parts of reinforcing agent, 60 parts of water reducing agent, 150 parts of silica brick powder, 30 parts of peat soil, 25 parts of defoaming agent and 750 parts of water;

[0070] S2, adding water to the silica brick powder and mixing, pouring it into the block-shaped mold, sending it to be fired, and processing the silica brick powder into the shape of the mold;

[0071] S3, adding peat soil into the material prepared in step S2 to fill the middle hole;

[0072] S4, pouring cement, limestone, fly ash and water into a mixing device for mixing and mixing evenly;

[0073] S5. During the stirring process, the reinforcing agent, water reducing agent and defoaming agent are continuously added and mixed and stirred;

[0074] S6. Filling aggregate on top of the material prepared in step S3;

[0075] S7, pouring the concrete mixed in step S5 onto the top of the aggregate for molding, and using a rolling device to continuously roll the upper surface to improve compactness;

[0076] S8. The formed ecological concrete is cured. After the curing is completed, the concrete is removed from the mold to complete the preparation.

[0077] The above-described embodiments are only preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various changes may be made to the above-described embodiments of the present invention. That is, any simple, equivalent changes and modifications made according to the claims and the contents of the specification of the present invention shall fall within the protection scope of the claims of the present invention. The conventional technical contents are not described in detail in the present invention.

[0078] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0079] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A production process of ecological concrete, It is characterized in that The production steps are: S1. Prepare the following raw materials: 10-500 parts of cement, 20-200 parts of limestone, 100-800 parts of fly ash, 200-600 parts of aggregate, 20-100 parts of reinforcing agent, 1-60 parts of water reducing agent, 1-200 parts of silica brick powder, 20-300 parts of peat soil, 1-50 parts of defoaming agent and 100-2000 parts of water; S2, adding water to silica brick powder and mixing, pouring into the block-shaped mold, sending it to be fired, and processing the silica brick powder into the shape of the mold; S3, adding peat soil into the material prepared in step S2 to fill the middle hole; S4, pouring cement, limestone, fly ash and water into a mixing device for mixing and mixing evenly; S5. During the stirring process, the reinforcing agent, water reducing agent and defoaming agent are continuously added and mixed and stirred; S6. Filling aggregate on top of the material prepared in step S3; S7, pouring the concrete mixed in step S5 onto the top of the aggregate for molding, and using a rolling device to continuously roll the upper surface to improve compactness; S8. The formed ecological concrete is cured. After the curing is completed, the concrete is removed from the mold to complete the preparation.

2. The production process of ecological concrete according to claim 1, Features: In step S2, the shape of the mold is a cube with a hollowed-out middle. The firing time is 5 hours. In step S3, the middle of the mold is filled and pressed to be compact. In step S4, the stirring time is 2 hours and the stirring speed is 30 r / min.

3. The production process of ecological concrete according to claim 1, Features: In step S5, after stirring in the stirring equipment for 30 minutes, a reinforcing agent is added into the stirring equipment, after stirring in the stirring equipment for 1.5 hours, a water reducing agent is added into the stirring equipment, after stirring in the stirring equipment for 1.8 hours, a defoaming agent is added into the stirring equipment, the aggregate selected in step S6 is crushed stone, the thickness of the aggregate layer is 50 mm, and the curing time in step S8 is 3 days.

4. An ecological concrete, It is characterized in that The ecological concrete is prepared by the production process of an ecological concrete described in any one of claims 1 to 3, and the ecological concrete comprises the following materials: 10-500 parts of cement, 20-200 parts of limestone, 100-800 parts of fly ash, 200-600 parts of aggregate, 20-100 parts of reinforcing agent, 1-60 parts of water reducing agent, 1-200 parts of silica brick powder, 20-300 parts of peat soil, 1-50 parts of defoaming agent and 100-2000 parts of water.

5. The ecological concrete according to claim 4, Features: 450 parts of cement, 100 parts of limestone, 150 parts of fly ash, 540 parts of aggregate, 80 parts of reinforcing agent, 40 parts of water reducing agent, 150 parts of silica brick powder, 220 parts of peat soil, 25 parts of defoaming agent and 1000 parts of water.

6. The ecological concrete according to claim 4, Features: The type of cement is one of silicate cement, aluminate cement and sulphoaluminate cement. The preparation steps of cement are as follows: prepare cement quartz, limestone and clay; the raw materials are crushed in the cement plant, and large pieces of quartz, limestone and clay are ground into powder respectively, and the equipment used is a hammer crusher; the quartz powder, limestone powder and clay powder are mixed according to a predetermined ratio to obtain a new material; the mixture is put into a rotary kiln and fired at a high temperature of 1400-1500°C in the rotary kiln. During the firing, the quartz and limestone react chemically under high temperature conditions and combine to form cement solids; after the firing is completed, the cement solids are gradually cooled and discharged from the top of the rotary kiln. The discharged cement solids are then crushed, screened and graded to obtain cement products of standard specifications.

7. The ecological concrete according to claim 4, Features: The limestone is one of high-calcium limestone, low-calcium limestone and mud limestone. The preparation steps of limestone are to mine limestone ore by blasting, crush the mined limestone ore, crush large pieces of limestone into smaller particles, place the particles in a lime kiln for calcining, grind the calcined material to obtain limestone, wherein the ratio of cement to limestone is 4.5:

1.

8. The ecological concrete according to claim 4, Features: Fly ash is one of bituminous coal fly ash, bituminous coal peat ash and anthracite fly ash. The preparation steps of fly ash are to select coal suitable for producing fly ash, crush and grind the selected coal to achieve the required fineness, burn the crushed fly ash through combustion equipment to generate high-temperature flue gas and ash, and the generated high-temperature flue gas is treated by dust collector and desulfurization equipment to remove dust and harmful gases. The ash generated after combustion is treated with dust collector for dust removal and centralized collection. Aggregates include sand, gravel, crushed stone, slag and concrete. The ratio of fly ash to aggregate is 1.5:5.

4.

9. The ecological concrete according to claim 4, Features: The enhancer is a silicate enhancer. The preparation steps of the enhancer are to prepare silicate, cement and gypsum raw materials; according to the prescribed formula ratio, the raw materials are put into a mixer for mixing and stirring, stirring evenly, adding an appropriate amount of water or other additives, adjusting the consistency of the silicate enhancer, and storing the prepared silicate enhancer in a dry and cool environment to avoid direct sunlight and moisture. The preparation steps of the water reducer are to add various raw materials into a mixing device, ensure that the quality and proportion of the raw materials meet the production requirements, fully stir and mix evenly, The mixed ingredients are filtered through a filtering device to remove impurities and solid particles therein, and dehydrated. The filtered and dehydrated ingredients are ground, and the ground raw materials are sent to a reactor, and a certain solvent and catalyst are added to synthesize a water reducer through reaction.

10. The ecological concrete according to claim 4, Features: The silica brick powder is obtained by crushing silica bricks, the peat soil is sphagnum peat soil, and the preparation step of the defoamer is to react alcohol with sulfuric acid to obtain ether. This reaction needs to be carried out in an acidic environment and needs to be heated to promote the reaction. After the reaction is completed, the ether is extracted from the reaction mixture by distillation; Oxidize n-octane to obtain octanal, then reduce octanal to obtain octanol, add sodium sulfate into a mixer, add silicone emulsion thereto, and stir evenly; then add sodium sulfate thereto, stir evenly, add silicone emulsion, stir evenly, add sodium citrate and maleic acid acrylic acid copolymer, continue stirring, add anhydrous ethanol and deionized water after stirring evenly, stir evenly, and then granulate and dry the obtained mixture.

Citation Information

Patent Citations

  • Siliceous refractory mortar with excellent high-temperature performance

    CN111548171A

  • Ecological concrete water permeable brick based on fly ash lightweight aggregate and preparation method thereof

    CN112500084A

  • High-strength recycled concrete and production process thereof

    CN113387622A

  • Preparation method of recycled brick vegetation concrete slope protection material

    CN113548818A

  • Heat-resistant and corrosion-resistant lightweight foam concrete and preparation method thereof

    CN115304336A