Method for preparing anti-skid and anti-penetration sole material

The combination of layered titanium dioxide and carbon nanotube composite fillers and phenolic resin modified rubber solves the problem of insufficient anti-slip performance of sole materials when punctured by sharp objects and in humid environments, achieving anti-slip, anti-odor and anti-penetration effects. Improves the overall protective performance of the sole.

CN117820737BActive Publication Date: 2024-10-25HUIZHOU SHENGBANG SHOES IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311580757.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-25
Estimated Expiration
2043-04-06

AI Technical Summary

Technical Problem

Existing sole materials are easily punctured when they come into contact with sharp objects and cannot effectively protect them, causing the penetration of toxic and harmful substances. They also have insufficient anti-slip properties in humid environments, making it difficult to prevent sliding and bacterial growth.

Method used

Composite fillers made of layered titanium dioxide and carbon nanotubes are used to coat phenolic resin and modified rubber, which are mixed and vulcanized to produce anti-slip and anti-penetration sole materials. Through the combination of modified rubber and phenolic resin, a multi-level ordered structure is formed. Enhance the anti-slip, anti-odor and anti-penetration properties of the sole.

Benefits of technology

It achieves the anti-slip, anti-odor and anti-penetration effects of the sole material, improves the puncture resistance and protective performance of the sole, enhances the blocking effect on sharp objects, and reduces bacterial growth and odor generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a method for preparing a non-slip and anti-penetration sole material, and relates to the technical field of soles. The present invention first inserts carbon nanotubes into layered titanium dioxide, which can absorb and penetrate external force energy, and then uses 4-chloromethyl-D-phenylalanine, dicyandiamide, and 3-(chloromethyl)-4-hydroxy-5-methoxy-benzaldehyde for modification, effectively reducing microbial activity, inhibiting the generation of malodorous substances, and then polymerizing the surface molecules of the composite filler to form a phenolic resin coated on the composite filler, which is conducive to improving the anti-slip ability of the sole; then 2,2'-diaminodiphenyl disulfide, dibromopropane, and 4,4-dihydroxybenzophenone are used to modify epoxy rubber, which can self-repair the penetration part, while increasing the rubber volume effect and the viscous effect and the intermolecular force, so that the sole is not easily pierced and broken. The sole material prepared by the present invention has the effects of non-slip, anti-penetration, and deodorization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of soles, in particular to a method for preparing an anti-skid and anti-penetration sole material. Background Art

[0002] Shoes are something we all wear, and the soles are an indispensable part of making shoes. In the process of daily walking, we often encounter sharp objects such as stones and needles. When the sole material comes into contact with sharp objects, it is very easy for the molecular chain to slip and break, and the sole is punctured. If it cannot effectively resist the puncture and puncture of sharp objects, it will not play a protective role, resulting in toxic and harmful substances infiltrating into the shoes, causing harm to the human body.

[0003] Anti-skid is the most important function of the sole, which can effectively protect the user from falling and slipping. Especially for the humid and oily working environment such as the hull deck and kitchen, excellent anti-skid performance is the safety guarantee for the user. In addition, shoes are a long-term closed environment, which is very easy to breed bacteria and microorganisms, leading to the generation of odor. Summary of the invention

[0004] The object of the present invention is to provide a non-slip and non-penetration sole material and a preparation method thereof, so as to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a non-slip and non-penetration sole material, wherein the non-slip and non-penetration sole material is prepared by preparing a composite filler from layered titanium dioxide and carbon nanotubes, coating the composite filler with phenolic resin, and mixing and vulcanizing the composite filler with modified rubber.

[0006] Furthermore, the phenolic resin is prepared by reacting 4-chloromethyl-D-phenylalanine, dicyandiamide, 3-(chloromethyl)-4-hydroxy-5-methoxy-benzaldehyde and phenol.

[0007] Furthermore, the modified rubber is prepared from epoxidized natural rubber, 2,2'-diaminodiphenyl disulfide, dibromopropane and 4,4-dihydroxybenzophenone.

[0008] Furthermore, a method for preparing an anti-slip and anti-penetration sole material comprises the following preparation steps:

[0009] (1) The composite filler, dichloromethane, 4-chloromethyl-D-phenylalanine, carbodiimide, and 4-dimethylaminopyridine were mixed in a mass ratio of 1:9:0.3:0.7:0.08 to 1:13:0.5:0.7:0.08, stirred at 60 rpm for 6 to 9 hours, and then dichloromethane 7 to 9 times the mass of the composite filler was added. After stirring for 20 minutes, the mixture was filtered, washed with deionized water and saturated brine for 4 to 6 times, and dried at 50°C for 4 hours to obtain the esterified filler;

[0010] (2) The esterified filler, hydrochloric acid (mass fraction: 0.8%) and dicyandiamide were mixed in a mass ratio of 1:30:0.5 to 1:40:1.2, stirred evenly, placed in a microwave oven, irradiated at 700 W for 18 to 30 min, cooled to room temperature, filtered, and the filter cake was washed with anhydrous ethanol for 4 to 6 times, and dried at 55 ° C for 6 h to obtain a guanidine-based filler;

[0011] (3) 3-(chloromethyl)-4-hydroxy-5-methoxy-benzaldehyde, guanidine filler, glacial acetic acid and chloroform were mixed in a mass ratio of 1:0.2:0.005:98 to 1:0.4:0.005:110, reacted at 60°C for 6 to 8 hours, and then anhydrous ethanol in an amount of 1754 times the mass of the guanidine filler was added. After standing for 30 minutes, the mixture was filtered to obtain a deodorizing filler.

[0012] (4) Under a nitrogen atmosphere, the deodorizing filler, methanol, phenol, and 37% hydrochloric acid are mixed in a mass ratio of 1:0.1:1.0:0.1 to 1:0.1:1.3:0.1, reacted at 90° C. for 4 to 6 hours, then heated to 180° C., decompressed to a pressure of 50 to 60 Pa, and distilled for 1 to 2 hours to obtain a phenolic resin filler;

[0013] (5) Dissolve the epoxidized rubber in toluene at a mass of 15 times the mass of the epoxidized rubber, stir until dissolved, add 2,2'-diaminodiphenyl disulfide at a mass of 0.2 to 0.4 times the mass of the epoxidized rubber, react at 50°C for 2 to 3 hours, add dibromopropane solution at a mass of 1.4 to 3.0 times the mass of the epoxidized rubber, the mass ratio of dibromopropane to toluene in the dibromopropane solution being 1:6, heat to 80°C, react for 2 to 4 hours, then add 4-diaminodiphenyl disulfide at a mass of 7 to 11 times the mass of the epoxidized rubber. Hydroxybenzophenone solution, anhydrous potassium carbonate 1.4 times the mass of epoxidized rubber, 4,4-dihydroxybenzophenone solution with a mass ratio of 1:4 to toluene, heated to 90°C, reacted under nitrogen atmosphere for 18-24 hours, added ultrapure water to pH 7, then added isopropanol solution 4-5 times the mass of epoxidized rubber, the mass ratio of isopropanol to glacial acetic acid in the isopropanol solution was 1:0.0005, 350nm, 3-4mW / cm 2 After irradiation for 6 days, add ultrapure water 100 times the mass of the epoxidized rubber, react at a vacuum degree of -0.06MPa and 68℃ for 7-9h, and dry at 50℃ for 4h to obtain the modified rubber;

[0014] (6) The modified rubber and styrene-butadiene rubber are respectively put into an open mill, and plasticized at 50-60° C. for 6-8 minutes. Then, the plasticized modified rubber and styrene-butadiene rubber are mixed in a mass ratio of 20:10-40:15. After mixing at 50-60° C. for 10-15 minutes, phenolic resin filler, stearic acid, and antioxidant 4010 are added in a mass ratio of 10:1:0.5-18:2:1, and the mass ratio of the modified rubber to the phenolic resin filler is 20:10-40:18. The temperature is raised to 70-80° C., and after mixing for 10-15 minutes, sulfur and accelerator M are added in a mass ratio of 1:1-3:2, and the mass ratio of the modified rubber to sulfur is 20:1-40:3. After vulcanization at 140-160° C. for 8-10 minutes, the anti-skid and anti-penetration sole material is obtained by molding.

[0015] Furthermore, the preparation method of the composite filler in step (1) is as follows: titanium dispersion and carbon nanotube dispersion are mixed in a mass ratio of 1:0.5 to 1:1.0, ultrasonically treated at 25 kHz for 30 minutes, and then 0.06 times the mass of triethylamine of the titanium dispersion is added. After ultrasonic homogenization, the mixture is reacted at 120° C. for 5 to 6 hours, washed with anhydrous ethanol for 7 to 9 times, and freeze-dried at -30° C. and a vacuum degree of 30 Pa for 7 to 9 hours to obtain the composite filler.

[0016] Furthermore, the titanium dispersion is a mixture of pretreated layered titanium dioxide and N,N-dimethylformamide in a mass ratio of 1:948, and ultrasonically treated at 25kHz for 30 minutes; the carbon nanotube dispersion is a mixture of carboxylated carbon nanotubes and N,N-dimethylformamide in a mass ratio of 1:948, and ultrasonically treated at 25kHz for 30 minutes.

[0017] Furthermore, the preparation method of the pretreated layered titanium dioxide is: layered titanium dioxide, KH560, and toluene are mixed in a mass ratio of 1:2:100 to 1:4:200, stirred at 120°C and 60rpm for 4 to 5 hours, washed with anhydrous ethanol for 3 to 5 hours, and dried at 60°C and a vacuum degree of 70kPa for 12 hours to obtain the pretreated layered titanium dioxide.

[0018] Furthermore, the preparation method of the layered titanium dioxide is as follows: dissolve titanium sulfate in distilled water with a mass of 20.8 times that of titanium sulfate, add ammonia water until the solution pH is 8-9, centrifuge at 3000-3500rpm for 20min, filter, wash with distilled water 4-6 times, add distilled water with a mass of 20.8 times that of titanium sulfate, stir at 60-80rpm for 10min, add hexadecyltrimethylammonium bromide with a mass of 0.05-0.07 times that of titanium sulfate, continue stirring for 20min, add 30% hydrogen peroxide with a mass fraction of 1.9 times that of titanium sulfate, continue stirring for 1h, age for 12h, dry at 80°C for 12h, grind until it passes through a 50-70 mesh sieve, place in a muffle furnace, and calcine at 500-600°C for 2h to obtain layered titanium dioxide.

[0019] Furthermore, the preparation method of the carboxylated carbon nanotubes is: disperse the carbon nanotubes in hydrogen peroxide with a mass fraction of 14630 times that of the carbon nanotubes, ultrasonically oscillate at 80-100W for 60 minutes, add sulfuric acid with a mass fraction of 6.2% with a mass fraction of 2080 times that of the carbon nanotubes, react at 100°C for 50-70 minutes, filter, wash with distilled water until the pH of the washing liquid is 7, and dry at 50°C for 5 hours to obtain the carboxylated carbon nanotubes.

[0020] Furthermore, the preparation method of the epoxidized rubber in step (5) is as follows: natural rubber and toluene are mixed in a mass ratio of 1:14 to 1:16, stirred at 70°C and 220 rpm until dissolved, deionized water is added to a solid content of 6%, and then formic acid in an amount of 1.5 to 2.0 times the mass of the natural rubber and hydrogen peroxide in an amount of 2.5 to 3.0 times the mass of the natural rubber are added, reacted at 50°C for 2 to 3 hours, anhydrous ethanol is added until precipitation is complete, filtered, washed with deionized water until the pH of the washing solution is 7, and dried at 30°C and a vacuum degree of -0.06 MPa for 2 hours to obtain the epoxidized rubber.

[0021] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0022] The present invention uses layered titanium dioxide and carbon nanotubes to prepare a composite filler, which is then coated with phenolic resin, mixed with modified rubber, and vulcanized to prepare a sole material to achieve the effects of anti-slip, anti-odor, and anti-penetration.

[0023] First, after the layered titanium dioxide is modified by KH56, its epoxy group reacts with the carboxylated carbon nanotubes to generate hydroxyl groups, and the two-dimensional layered structure is combined with the one-dimensional carbon nanotube array to form a multi-level ordered three-dimensional carbon nanotube intercalation structure, which increases the roughness of the sole while having a certain resilience, can absorb the energy of the piercing external force, and make the sole less likely to be pierced; 4-chloromethyl-D-phenylalanine is grafted on the surface of the composite filler using the carboxyl group, and its amino group reacts with dicyandiamide to form a guanidine group, which effectively inhibits the activity of microorganisms and the production of odorous substances, thereby improving the deodorizing effect of the sole material; the amino group in the guanidine group reacts with 3-(chloromethyl)-4-hydroxy-5- The aldehyde group of methoxy-benzaldehyde reacts to form a Schiff base group, which works together with the guanidine group and titanium dioxide to improve the antibacterial effect of the sole material, thereby improving the deodorizing ability; the chloromethylbenzene at both ends of the molecular chain on the surface of the composite filler reacts with phenol to form a phenolic resin that is coated on the composite filler, increasing the interaction between the surface of the composite filler and water molecules, reducing the thickness of the water film between the micro-convexities on the sole surface and the ground, and increasing the area and friction of the wet contact surface; at the same time, the phenolic resin introduces polar phenolic hydroxyl and benzene ring structures, which have good compatibility with modified rubber and are beneficial to increasing the glass transition temperature of the rubber system, so as to increase the hysteresis friction of the sole, thereby enhancing the anti-slip ability.

[0024] Secondly, after the rubber is epoxidized, the amino group of 2,2'-diaminodiphenyl disulfide reacts with the epoxy group, and a thermally reversible group is introduced into the rubber molecular chain, which can self-repair the penetrated part, making the sole material have an anti-penetration effect; under the bridging effect of dibromopropane, 2,2'-diaminodiphenyl disulfide reacts with 4,4-dihydroxybenzophenone, and then 4,4-dihydroxybenzophenone relies on the ketone group to form a glycol ethane structure with isopropanol, which contains a photoreversible carbon-carbon bond, so that the sole material can self-repair when exposed to light and improve the anti-penetration ability. At the same time, hydroxyl groups, benzene rings and other groups are introduced into the rubber molecular chain to increase the volume of the rubber. The elastic effect and viscosity effect can form an effective blocking effect on sharp objects in contact with the outside world, and can also increase the intermolecular force. Under the action of external force, it is easy to produce tensile crystallization, and the molecules are not easy to slip, so it is not easy to be pierced or broken. In addition, under the action of phenolic resin, the composite filler is evenly dispersed in the modified rubber to form a high-strength reinforcement network. When the sole is subjected to piercing external force, the reinforcement network can play a good blocking role. At the same time, the intercalated modified titanium dioxide of carbon nanotubes greatly improves the photothermal conversion ability of the composite filler, strengthens the photothermal repair effect of the modified rubber, and enhances the anti-penetration property of the sole material. DETAILED DESCRIPTION

[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0026] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the anti-slip and anti-penetration sole materials prepared in the following examples are as follows:

[0027] Anti-slip property: The friction coefficients of the embodiments and comparative examples of the same size were tested in dry and wet conditions according to GB / T 3903.6.

[0028] Penetration resistance: Take the same size of the embodiment and the comparative example and refer to GB / T 28288 to test the maximum force value of the sole material puncture, and after puncturing with a needle, irradiate with 365nm ultraviolet light for 20 minutes at 25℃, measure the depth of the hole after repair, and calculate the self-repair efficiency; self-repair efficiency = (hole depth before repair-hole depth after repair) / hole depth after repair.

[0029] Deodorization: The antibacterial rates of the embodiment and the comparative example of the same size were tested against Staphylococcus aureus and Candida albicans according to QB / T 2881.

[0030] Example 1

[0031] (1) Dispersing carbon nanotubes in hydrogen peroxide (14630 times the mass of carbon nanotubes), 80W ultrasonic oscillation for 60 min, adding 6.2% sulfuric acid (2080 times the mass of carbon nanotubes), reacting at 100°C for 50 min, filtering, washing with distilled water until the pH of the washing solution is 7, and drying at 50°C for 5 h to obtain carboxylated carbon nanotubes;

[0032] (2) Dissolve titanium sulfate in distilled water with a mass of 20.8 times that of titanium sulfate, add ammonia water until the solution pH is 8, centrifuge at 3000rpm for 20min, filter, wash with distilled water 4 times, add distilled water with a mass of 20.8 times that of titanium sulfate, stir at 60rpm for 10min, add hexadecyltrimethylammonium bromide with a mass of 0.05 times that of titanium sulfate, continue stirring for 20min, add hydrogen peroxide with a mass fraction of 30% with a mass of 1.9 times that of titanium sulfate, continue stirring for 1h, age for 12h, dry at 80℃ for 12h, grind until it passes through a 50-mesh sieve, place in a muffle furnace, and calcine at 500℃ for 2h to obtain layered titanium dioxide; mix layered titanium dioxide, KH560, and toluene in a mass ratio of 1:2:100, stir at 120℃ and 60rpm for 4h, wash with anhydrous ethanol for 3 times, and dry at 60℃ and a vacuum degree of 70kPa for 12h to obtain pretreated layered titanium dioxide;

[0033] (3) Pretreated layered titanium dioxide and N,N-dimethylformamide were mixed at a mass ratio of 1:948, and ultrasonic treatment was performed at 25kHz for 30 minutes to obtain a titanium dispersion; carboxylated carbon nanotubes and N,N-dimethylformamide were mixed at a mass ratio of 1:948, and ultrasonic treatment was performed at 25kHz for 30 minutes to obtain a carbon nanotube dispersion; the titanium dispersion and the carbon nanotube dispersion were mixed at a mass ratio of 1:0.5, and ultrasonic treatment was performed at 25kHz for 30 minutes, and then 0.06 times the mass of triethylamine of the titanium dispersion was added, and after ultrasonic homogenization, the mixture was reacted at 120°C for 5 hours, washed with anhydrous ethanol for 7 times, and freeze-dried at -30°C and a vacuum degree of 30Pa for 7 hours to obtain a composite filler;

[0034] (4) The composite filler, dichloromethane, 4-chloromethyl-D-phenylalanine, carbodiimide, and 4-dimethylaminopyridine were mixed in a mass ratio of 1:9:0.3:0.7:0.08, stirred at 60 rpm for 6 h, and then dichloromethane 7 times the mass of the composite filler was added. The mixture was stirred for 20 min, filtered, washed with deionized water and saturated brine 4 times in sequence, and dried at 50 °C for 4 h to obtain the esterified filler;

[0035] (5) The esterified filler, hydrochloric acid (mass fraction: 0.8%) and dicyandiamide were mixed in a mass ratio of 1:30:0.5, stirred evenly, placed in a microwave oven, irradiated at 700 W for 18 min, cooled to room temperature, filtered, and the filter cake was washed with anhydrous ethanol for 4 times, and dried at 55 ° C for 6 h to obtain a guanidine-based filler;

[0036] (6) 3-(chloromethyl)-4-hydroxy-5-methoxy-benzaldehyde, guanidine filler, glacial acetic acid and chloroform were mixed in a mass ratio of 1:0.2:0.005:98, reacted at 60°C for 6 hours, and then anhydrous ethanol 1754 times the mass of the guanidine filler was added. After standing for 30 minutes, the mixture was filtered to obtain a deodorizing filler.

[0037] (7) Under nitrogen atmosphere, the deodorizing filler, methanol, phenol, and 37% hydrochloric acid were mixed in a mass ratio of 1:0.1:1.0:0.1, reacted at 90°C for 4 hours, then heated to 180°C, decompressed to 50 Pa, and distilled for 1 hour to obtain a phenolic resin filler;

[0038] (8) Natural rubber and toluene were mixed in a mass ratio of 1:14, stirred at 70°C and 220 rpm until dissolved, deionized water was added until the solid content was 6%, and then formic acid (1.5 times the mass of natural rubber) and hydrogen peroxide (2.5 times the mass of natural rubber) were added. After reacting at 50°C for 2 h, anhydrous ethanol was added until precipitation was complete, filtered, washed with deionized water until the pH of the washing solution was 7, and dried at 30°C and a vacuum degree of -0.06 MPa for 2 h to obtain the epoxidized rubber;

[0039] (9) Dissolve the epoxidized rubber in toluene (15 times the mass of the epoxidized rubber), stir until dissolved, add 2,2'-diaminodiphenyl disulfide (0.2 times the mass of the epoxidized rubber), react at 50°C for 2 h, add dibromopropane solution (1.4 times the mass of the epoxidized rubber), the mass ratio of dibromopropane to toluene in the dibromopropane solution is 1:6, heat to 80°C, react for 2 h, add 4-dihydroxybenzophenone solution (7 times the mass of the epoxidized rubber) and anhydrous potassium carbonate (1.4 times the mass of the epoxidized rubber), the mass ratio of 4,4-dihydroxybenzophenone to toluene in the 4,4-dihydroxybenzophenone solution is 1:4, heat to 90°C, react under nitrogen atmosphere for 18 h, add ultrapure water to pH 7, then add isopropanol solution (4 times the mass of the epoxidized rubber), the mass ratio of isopropanol to glacial acetic acid in the isopropanol solution is 1:0.0005, 350 nm, 3 mW / cm 2 After irradiation for 6 days, add ultrapure water 100 times the mass of the epoxidized rubber, react at a vacuum degree of -0.06MPa and 68℃ for 7h, and then dry at 50℃ for 4h to obtain the modified rubber;

[0040] (10) The modified rubber and styrene-butadiene rubber were respectively put into an open mill and plasticized at 50°C for 6 min. The plasticized modified rubber and styrene-butadiene rubber were then mixed in a mass ratio of 20:10. After mixing at 50°C for 10 min, phenolic resin filler, stearic acid and antioxidant 4010 were added in a mass ratio of 10:1:0.5 (the mass ratio of the modified rubber to the phenolic resin filler was 20:10). The temperature was raised to 70°C and mixed for 10 min. Then, sulfur and accelerator M were added in a mass ratio of 1:1 (the mass ratio of the modified rubber to sulfur was 20:1). After vulcanization at 140°C for 8 min, the anti-skid and anti-penetration sole material was obtained by molding.

[0041] Example 2

[0042] (1) Dispersing carbon nanotubes in hydrogen peroxide (14630 times the mass of carbon nanotubes), oscillating at 90W ultrasonic for 60 min, adding sulfuric acid (2080 times the mass of carbon nanotubes) with a mass fraction of 6.2%, reacting at 100°C for 60 min, filtering, washing with distilled water until the pH of the washing solution is 7, and drying at 50°C for 5 h to obtain carboxylated carbon nanotubes;

[0043] (2) Dissolve titanium sulfate in distilled water with a mass of 20.8 times that of titanium sulfate, add ammonia water until the solution pH is 8.5, centrifuge at 3300rpm for 20min, filter, wash with distilled water 5 times, add distilled water with a mass of 20.8 times that of titanium sulfate, stir at 70rpm for 10min, add hexadecyltrimethylammonium bromide with a mass of 0.06 times that of titanium sulfate, continue stirring for 20min, add 30% hydrogen peroxide with a mass fraction of 1.9 times that of titanium sulfate, continue stirring for 1h, age for 12h, dry at 80℃ for 12h, grind until it passes through a 60-mesh sieve, place in a muffle furnace, and calcine at 550℃ for 2h to obtain layered titanium dioxide; mix layered titanium dioxide, KH560, and toluene in a mass ratio of 1:3:150, stir at 120℃ and 60rpm for 4.5h, wash with anhydrous ethanol for 4, and dry at 60℃ and a vacuum degree of 70kPa for 12h to obtain pretreated layered titanium dioxide;

[0044] (3) Pretreated layered titanium dioxide and N,N-dimethylformamide were mixed at a mass ratio of 1:948, and ultrasonic treatment was performed at 25kHz for 30 minutes to obtain a titanium dispersion; carboxylated carbon nanotubes and N,N-dimethylformamide were mixed at a mass ratio of 1:948, and ultrasonic treatment was performed at 25kHz for 30 minutes to obtain a carbon nanotube dispersion; the titanium dispersion and the carbon nanotube dispersion were mixed at a mass ratio of 1:0.75, and ultrasonic treatment was performed at 25kHz for 30 minutes, and then 0.06 times the mass of triethylamine of the titanium dispersion was added, and after ultrasonic homogenization, the mixture was reacted at 120°C for 5.5 hours, washed with anhydrous ethanol for 8 times, and freeze-dried at -30°C and a vacuum degree of 30Pa for 8 hours to obtain a composite filler;

[0045] (4) The composite filler, dichloromethane, 4-chloromethyl-D-phenylalanine, carbodiimide, and 4-dimethylaminopyridine were mixed in a mass ratio of 1:11:0.4:0.7:0.08, stirred at 60 rpm for 7.5 h, and then 8 times the mass of the composite filler was added with dichloromethane. The mixture was stirred for 20 min, filtered, washed with deionized water and saturated brine for 5 times, and dried at 50 °C for 4 h to obtain the esterified filler;

[0046] (5) The esterified filler, hydrochloric acid (mass fraction: 0.8%) and dicyandiamide were mixed in a mass ratio of 1:35:0.85, stirred evenly, placed in a microwave oven, irradiated at 700 W for 24 min, cooled to room temperature, filtered, and the filter cake was washed with anhydrous ethanol for 5 times, and dried at 55 ° C for 6 h to obtain a guanidine-based filler;

[0047] (6) 3-(chloromethyl)-4-hydroxy-5-methoxy-benzaldehyde, guanidine filler, glacial acetic acid and chloroform were mixed in a mass ratio of 1:0.3:0.005:104, reacted at 60°C for 7 hours, and then anhydrous ethanol 1754 times the mass of the guanidine filler was added. After standing for 30 minutes, the mixture was filtered to obtain a deodorizing filler.

[0048] (7) Under nitrogen atmosphere, the deodorizing filler, methanol, phenol, and 37% hydrochloric acid were mixed in a mass ratio of 1:0.1:1.15:0.1, reacted at 90°C for 5 hours, then heated to 180°C, decompressed to 55 Pa, and distilled for 1.5 hours to obtain a phenolic resin filler;

[0049] (8) Natural rubber and toluene were mixed in a mass ratio of 1:15, stirred at 70°C and 220 rpm until dissolved, deionized water was added until the solid content was 6%, and then formic acid (1.75 times the mass of natural rubber) and hydrogen peroxide (2.75 times the mass of natural rubber) were added. After reacting at 50°C for 2.5 hours, anhydrous ethanol was added until precipitation was complete, filtered, washed with deionized water until the pH of the washing solution was 7, and dried at 30°C and a vacuum degree of -0.06 MPa for 2 hours to obtain the epoxidized rubber;

[0050] (9) Dissolve the epoxidized rubber in toluene (15 times the mass of the epoxidized rubber), stir until dissolved, add 2,2'-diaminodiphenyl disulfide (0.3 times the mass of the epoxidized rubber), react at 50°C for 2.5 hours, add dibromopropane solution (2.2 times the mass of the epoxidized rubber), the mass ratio of dibromopropane to toluene in the dibromopropane solution is 1:6, heat to 80°C, react for 3 hours, add 4-dihydroxybenzophenone solution (9 times the mass of the epoxidized rubber) and anhydrous potassium carbonate (1.4 times the mass of the epoxidized rubber), the mass ratio of 4,4-dihydroxybenzophenone to toluene in the 4,4-dihydroxybenzophenone solution is 1:4, heat to 90°C, react under nitrogen atmosphere for 21 hours, add ultrapure water to pH 7, then add isopropanol solution (4.5 times the mass of the epoxidized rubber), the mass ratio of isopropanol to glacial acetic acid in the isopropanol solution is 1:0.0005, 350 nm, 3.5 mW / cm 2 After irradiation for 6 days, add ultrapure water 100 times the mass of the epoxidized rubber, react at a vacuum degree of -0.06MPa and 68℃ for 8h, and then dry at 50℃ for 4h to obtain the modified rubber;

[0051] (10) The modified rubber and styrene-butadiene rubber were respectively put into an open mill and plasticized at 55° C. for 7 min. The plasticized modified rubber and styrene-butadiene rubber were then mixed in a mass ratio of 30:12.5. After mixing at 55° C. for 12 min, phenolic resin filler, stearic acid and antioxidant 4010 were added in a mass ratio of 14:1.5:0.75 (the mass ratio of the modified rubber to the phenolic resin filler was 30:14). The temperature was raised to 75° C. and mixed for 12 min. Then, sulfur and accelerator M were added in a mass ratio of 2:1.5 (the mass ratio of the modified rubber to sulfur was 30:2). After vulcanization at 150° C. for 9 min, the anti-skid and anti-penetration sole material was obtained by molding.

[0052] Example 3

[0053] (1) Dispersing carbon nanotubes in hydrogen peroxide (14630 times the mass of carbon nanotubes), ultrasonically oscillating at 100W for 60 minutes, adding sulfuric acid (2080 times the mass of carbon nanotubes) with a mass fraction of 6.2%, reacting at 100°C for 70 minutes, filtering, washing with distilled water until the pH of the washing solution is 7, and drying at 50°C for 5 hours to obtain carboxylated carbon nanotubes;

[0054] (2) Dissolve titanium sulfate in distilled water with a mass of 20.8 times the mass of titanium sulfate, add ammonia water until the solution pH is 9, centrifuge at 3500rpm for 20min, filter, wash with distilled water 6 times, add distilled water with a mass of 20.8 times the mass of titanium sulfate, stir at 80rpm for 10min, add hexadecyltrimethylammonium bromide with a mass of 0.07 times the mass of titanium sulfate, continue stirring for 20min, add hydrogen peroxide with a mass fraction of 30% with a mass of 1.9 times the mass of titanium sulfate, continue stirring for 1h, age for 12h, dry at 80℃ for 12h, grind until it passes through a 70-mesh sieve, place in a muffle furnace, and calcine at 600℃ for 2h to obtain layered titanium dioxide; mix layered titanium dioxide, KH560, and toluene in a mass ratio of 1:4:200, stir at 120℃ and 60rpm for 5h, wash with anhydrous ethanol for 5, and dry at 60℃ and a vacuum degree of 70kPa for 12h to obtain pretreated layered titanium dioxide;

[0055] (3) Pretreated layered titanium dioxide and N,N-dimethylformamide were mixed in a mass ratio of 1:948, and ultrasonic treatment was performed at 25kHz for 30 minutes to obtain a titanium dispersion; carboxylated carbon nanotubes and N,N-dimethylformamide were mixed in a mass ratio of 1:948, and ultrasonic treatment was performed at 25kHz for 30 minutes to obtain a carbon nanotube dispersion; the titanium dispersion and the carbon nanotube dispersion were mixed in a mass ratio of 1:1, and ultrasonic treatment was performed at 25kHz for 30 minutes, and then 0.06 times the mass of triethylamine of the titanium dispersion was added, and after ultrasonic homogenization, the mixture was reacted at 120°C for 6 hours, washed with anhydrous ethanol for 9 times, and freeze-dried at -30°C and a vacuum degree of 30Pa for 9 hours to obtain a composite filler;

[0056] (4) The composite filler, dichloromethane, 4-chloromethyl-D-phenylalanine, carbodiimide, and 4-dimethylaminopyridine were mixed in a mass ratio of 1:13:0.5:0.7:0.08, stirred at 60 rpm for 9 h, and then dichloromethane 9 times the mass of the composite filler was added. The mixture was stirred for 20 min, filtered, washed with deionized water and saturated brine for 6 times, and dried at 50 °C for 4 h to obtain the esterified filler;

[0057] (5) The esterified filler, hydrochloric acid (mass fraction: 0.8%) and dicyandiamide were mixed in a mass ratio of 1:40:1.2, stirred evenly, placed in a microwave oven, irradiated at 700 W for 30 min, cooled to room temperature, filtered, and the filter cake was washed with anhydrous ethanol for 6 times, and dried at 55 ° C for 6 h to obtain a guanidine-based filler;

[0058] (6) 3-(chloromethyl)-4-hydroxy-5-methoxy-benzaldehyde, guanidine filler, glacial acetic acid and chloroform were mixed in a mass ratio of 1:0.4:0.005:110, reacted at 60°C for 8 hours, and then anhydrous ethanol 1754 times the mass of the guanidine filler was added. After standing for 30 minutes, the mixture was filtered to obtain a deodorizing filler.

[0059] (7) Under nitrogen atmosphere, the deodorizing filler, methanol, phenol, and 37% hydrochloric acid were mixed in a mass ratio of 1:0.1:1.3:0.1, reacted at 90°C for 6 hours, then heated to 180°C, decompressed to 60 Pa, and distilled for 2 hours to obtain a phenolic resin filler;

[0060] (8) Natural rubber and toluene were mixed in a mass ratio of 1:16, stirred at 70°C and 220 rpm until dissolved, deionized water was added until the solid content was 6%, and then formic acid twice the mass of natural rubber and hydrogen peroxide three times the mass of natural rubber were added. After reacting at 50°C for 3 h, anhydrous ethanol was added until precipitation was complete, filtered, washed with deionized water until the pH of the washing solution was 7, and dried at 30°C and a vacuum degree of -0.06 MPa for 2 h to obtain the epoxidized rubber;

[0061] (9) Dissolve the epoxidized rubber in toluene (15 times the mass of the epoxidized rubber), stir until dissolved, add 2,2'-diaminodiphenyl disulfide (0.4 times the mass of the epoxidized rubber), react at 50°C for 3 h, add dibromopropane solution (3 times the mass of the epoxidized rubber), the mass ratio of dibromopropane to toluene in the dibromopropane solution is 1:6, heat to 80°C, react for 4 h, add 4-dihydroxybenzophenone solution (11 times the mass of the epoxidized rubber) and anhydrous potassium carbonate (1.4 times the mass of the epoxidized rubber), the mass ratio of 4,4-dihydroxybenzophenone to toluene in the 4,4-dihydroxybenzophenone solution is 1:4, heat to 90°C, react under nitrogen atmosphere for 24 h, add ultrapure water to pH 7, then add isopropanol solution (5 times the mass of the epoxidized rubber), the mass ratio of isopropanol to glacial acetic acid in the isopropanol solution is 1:0.0005, 350 nm, 4 mW / cm 2 After irradiation for 6 days, add ultrapure water 100 times the mass of the epoxidized rubber, react at a vacuum degree of -0.06MPa and 68℃ for 9 hours, and dry at 50℃ for 4 hours to obtain the modified rubber;

[0062] (10) The modified rubber and styrene-butadiene rubber were respectively put into an open mill and plasticized at 60°C for 8 minutes. The plasticized modified rubber and styrene-butadiene rubber were then mixed in a mass ratio of 40:15. After mixing at 60°C for 15 minutes, phenolic resin filler, stearic acid and antioxidant 4010 were added in a mass ratio of 18:2:1, and the mass ratio of the modified rubber to the phenolic resin filler was 40:18. The temperature was raised to 80°C and mixed for 15 minutes. Then, sulfur and accelerator M were added in a mass ratio of 3:2, and the mass ratio of the modified rubber to sulfur was 40:3. After vulcanization at 160°C for 10 minutes, the anti-skid and anti-penetration sole material was obtained by molding.

[0063] Comparative Example 1

[0064] The difference between Comparative Example 1 and Example 2 is that there are no steps (1) to (3), and step (4) is changed to: carbon nanotubes, dichloromethane, 4-chloromethyl-D-phenylalanine, carbodiimide, and 4-dimethylaminopyridine are mixed in a mass ratio of 1:11:0.4:0.7:0.08, stirred at 60 rpm for 7.5 hours, and then dichloromethane 8 times the mass of the carbon nanotubes is added, and stirred for 20 minutes, and then filtered, washed with deionized water and saturated brine for 5 times, and dried at 50° C. for 4 hours to obtain an esterified filler. The remaining steps are the same as those in Example 2.

[0065] Comparative Example 2

[0066] The difference between Comparative Example 2 and Example 2 is that step (4) is omitted, and step (5) is changed to: the composite filler, hydrochloric acid with a mass fraction of 0.8%, and dicyandiamide are mixed in a mass ratio of 1:35:0.85, stirred evenly, placed in a microwave oven, irradiated at 700 W for 24 min, cooled to room temperature, filtered, and the filter cake is taken, washed with anhydrous ethanol 5 times, and dried at 55° C. for 6 h to obtain a guanidine-based filler. The remaining steps are the same as those in Example 2.

[0067] Comparative Example 3

[0068] The difference between Comparative Example 3 and Example 2 is that there are no steps (6) and (7), and step (10) is changed to: the modified rubber and styrene-butadiene rubber are respectively put into an open mill, and plasticized at 55° C. for 7 minutes, and then the plasticized modified rubber and styrene-butadiene rubber are mixed in a mass ratio of 30:12.5, and after mixing at 55° C. for 12 minutes, guanidine filler, stearic acid, and antioxidant 4010 are added in a mass ratio of 14:1.5:0.75, and the mass ratio of the modified rubber to the phenolic resin filler is 30:14, the temperature is raised to 75° C., and after mixing for 12 minutes, sulfur and accelerator M are added in a mass ratio of 2:1.5, and the mass ratio of the modified rubber to sulfur is 30:2, and after vulcanization at 150° C. for 9 minutes, the anti-skid and anti-penetration sole material is obtained by molding. The remaining steps are the same as those of Example 2.

[0069] Comparative Example 4

[0070] The difference between Comparative Example 4 and Example 2 is that step (9) is changed to: dissolve the epoxidized rubber in toluene with a mass of 15 times that of the epoxidized rubber, stir until dissolved, add a dibromopropane solution with a mass of 2.2 times that of the epoxidized rubber, the mass ratio of dibromopropane to toluene in the dibromopropane solution is 1:6, heat to 80°C, react for 3 hours, add a 4-dihydroxybenzophenone solution with a mass of 9 times that of the epoxidized rubber and anhydrous potassium carbonate with a mass of 1.4 times that of the epoxidized rubber, the mass ratio of 4,4-dihydroxybenzophenone to toluene in the 4,4-dihydroxybenzophenone solution is 1:4, heat to 90°C, react for 21 hours under a nitrogen atmosphere, add ultrapure water to a pH of 7, and then add an isopropanol solution with a mass of 4.5 times that of the epoxidized rubber, the mass ratio of isopropanol to glacial acetic acid in the isopropanol solution is 1:0.0005, 350nm, 3.5mW / cm 2 After irradiation for 6 days, ultrapure water 100 times the mass of the epoxidized rubber was added, the reaction was carried out at a vacuum degree of -0.06 MPa and 68°C for 8 hours, and then dried at 50°C for 4 hours to obtain the modified rubber. The remaining steps were the same as those in Example 2.

[0071] Comparative Example 5

[0072] The difference between Comparative Example 5 and Example 2 is that step (9) is different. Step (9) is changed to: dissolve the epoxidized rubber in toluene with a mass of 15 times that of the epoxidized rubber, stir until dissolved, add 2,2'-diaminodiphenyl disulfide with a mass of 0.3 times that of the epoxidized rubber, react at 50°C for 2.5 hours, react at 68°C for 8 hours under a vacuum degree of -0.06 MPa, and dry at 50°C for 4 hours to obtain the modified rubber. The remaining steps are the same as those in Example 2.

[0073] Effect example

[0074] Table 1 below shows the performance analysis results of the anti-skid and anti-penetration sole materials of Examples 1 to 3 of the present invention and Comparative Examples 1 to 5.

[0075] Table 1

[0076]

[0077] From the comparison of the friction coefficient and antibacterial rate experimental data of the embodiment and the comparative example, it can be found that the layered titanium dioxide and carbon nanotubes constitute a rough sole surface, and are modified by using 4-chloromethyl-D-phenylalanine, dicyandiamide, and 3-(chloromethyl)-4-hydroxy-5-methoxy-benzaldehyde to generate multiple antibacterial groups, which work together with titanium dioxide to effectively inhibit the activity of microorganisms and the generation of odorous substances. Then, the molecules on the surface of the composite filler are polymerized to form a phenolic resin coated on the composite filler, which reduces the thickness of the water film between the micro-convex surface of the sole and the ground, improves the compatibility with the modified rubber, and is beneficial to increase the glass transition temperature of the rubber system to increase the hysteresis friction of the sole, thereby Enhanced anti-slip ability; from the comparison of the maximum force value and self-repair efficiency experimental data of the embodiment and the comparative example, it can be found that the present invention utilizes 2,2'-diaminodiphenyl disulfide, dibromopropane, and 4,4-dihydroxybenzophenone to modify epoxy rubber, introduces photothermal reversible groups, and can self-repair the penetrated part, while increasing the rubber volume effect and viscosity effect and the force between molecules, so that it is not easy to be pierced or broken; in addition, the intercalated modified titanium dioxide of carbon nanotubes greatly improves the photothermal conversion ability of the composite filler, strengthens the photothermal repair effect of the modified rubber, and under the action of phenolic resin, is evenly dispersed in the modified rubber to form a high-strength reinforcement network, thereby enhancing the anti-penetration property of the sole material.

[0078] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and range of equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing an anti-skid and anti-penetration sole material, characterized in that: The method comprises the following preparation steps: (1) Dispersing carbon nanotubes in hydrogen peroxide (14630 times the mass of carbon nanotubes), ultrasonically oscillating at 90W for 60 min, adding sulfuric acid (2080 times the mass of carbon nanotubes) with a mass fraction of 6.2%, reacting at 100°C for 60 min, filtering, washing with distilled water until the pH of the washing solution is 7, and drying at 50°C for 5 h to obtain carboxylated carbon nanotubes; (2) Dissolve titanium sulfate in distilled water with a mass of 20.8 times that of titanium sulfate, add ammonia water until the solution pH is 8.5, centrifuge at 3300 rpm for 20 min, filter, wash with distilled water 5 times, add distilled water with a mass of 20.8 times that of titanium sulfate, stir at 70 rpm for 10 min, add hexadecyltrimethylammonium bromide with a mass of 0.06 times that of titanium sulfate, continue stirring for 20 min, add 30% hydrogen peroxide with a mass fraction of 1.9 times that of titanium sulfate, continue stirring for 1 h, age for 12 h, dry at 80 ° C for 12 h, grind until it passes through a 60 mesh sieve, place in a muffle furnace, and calcine at 550 ° C for 2 h to obtain layered titanium dioxide; mix layered titanium dioxide, KH560, and toluene in a mass ratio of 1:3:150, stir at 120 ° C and 60 rpm for 4.5 h, wash with anhydrous ethanol 4 times, and dry at 60 ° C and a vacuum degree of 70 kPa for 12 h to obtain pretreated layered titanium dioxide; (3) Pretreated layered titanium dioxide and N,N-dimethylformamide were mixed at a mass ratio of 1:948, and ultrasonic treatment was performed at 25kHz for 30 minutes to obtain a titanium dispersion; carboxylated carbon nanotubes and N,N-dimethylformamide were mixed at a mass ratio of 1:948, and ultrasonic treatment was performed at 25kHz for 30 minutes to obtain a carbon nanotube dispersion; the titanium dispersion and the carbon nanotube dispersion were mixed at a mass ratio of 1:0.75, and ultrasonic treatment was performed at 25kHz for 30 minutes, and then 0.06 times the mass of triethylamine of the titanium dispersion was added, and after ultrasonic homogenization, the mixture was reacted at 120°C for 5.5 hours, washed with anhydrous ethanol for 8 times, and freeze-dried at -30°C and a vacuum degree of 30Pa for 8 hours to obtain a composite filler; (4) The composite filler, dichloromethane, 4-chloromethyl-D-phenylalanine, carbodiimide, and 4-dimethylaminopyridine were mixed in a mass ratio of 1:11:0.4:0.7:0.08, stirred at 60 rpm for 7.5 h, and then 8 times the mass of the composite filler was added with dichloromethane. The mixture was stirred for 20 min, filtered, washed with deionized water and saturated brine for 5 times, and dried at 50 °C for 4 h to obtain the esterified filler; (5) The esterified filler, hydrochloric acid (mass fraction: 0.8%) and dicyandiamide were mixed in a mass ratio of 1:35:0.85, stirred evenly, placed in a microwave oven, irradiated at 700 W for 24 min, cooled to room temperature, filtered, and the filter cake was washed with anhydrous ethanol for 5 times, and dried at 55 ° C for 6 h to obtain a guanidine-based filler; (6) 3-(chloromethyl)-4-hydroxy-5-methoxy-benzaldehyde, guanidine filler, glacial acetic acid and chloroform were mixed in a mass ratio of 1:0.3:0.005:104, reacted at 60°C for 7 hours, and then anhydrous ethanol 1754 times the mass of the guanidine filler was added. After standing for 30 minutes, the mixture was filtered to obtain a deodorizing filler. (7) Under nitrogen atmosphere, the deodorizing filler, methanol, phenol, and 37% hydrochloric acid were mixed in a mass ratio of 1:0.1:1.15:0.1, reacted at 90°C for 5 hours, then heated to 180°C, decompressed to 55 Pa, and distilled for 1.5 hours to obtain a phenolic resin filler; (8) Natural rubber and toluene were mixed in a mass ratio of 1:15, stirred at 70°C and 220 rpm until dissolved, deionized water was added until the solid content was 6%, and then formic acid (1.75 times the mass of natural rubber) and hydrogen peroxide (2.75 times the mass of natural rubber) were added. After reacting at 50°C for 2.5 hours, anhydrous ethanol was added until precipitation was complete, filtered, washed with deionized water until the pH of the washing solution was 7, and dried at 30°C and a vacuum degree of -0.06 MPa for 2 hours to obtain the epoxidized rubber; (9) Dissolve the epoxidized rubber in toluene (15 times the mass of the epoxidized rubber), stir until dissolved, add 2,2'-diaminodiphenyl disulfide (0.3 times the mass of the epoxidized rubber), react at 50°C for 2.5 hours, add dibromopropane solution (2.2 times the mass of the epoxidized rubber), the mass ratio of dibromopropane to toluene in the dibromopropane solution is 1:6, heat to 80°C, react for 3 hours, add 4-dihydroxybenzophenone solution (9 times the mass of the epoxidized rubber), anhydrous potassium carbonate (1.4 times the mass of the epoxidized rubber), and 4,4-dihydroxybenzophenone solution (1.4 times the mass of the epoxidized rubber). The mass ratio of 4,4-dihydroxybenzophenone and toluene in the benzophenone solution is 1:4, the temperature is raised to 90°C, and after reacting for 21 hours under a nitrogen atmosphere, ultrapure water is added to a pH of 7, and then an isopropanol solution of 4.5 times the mass of the epoxidized rubber is added, and the mass ratio of isopropanol and glacial acetic acid in the isopropanol solution is 1:0.0005. After irradiation at 350nm and 3.5mW / cm2 for 6 days, ultrapure water of 100 times the mass of the epoxidized rubber is added, the vacuum degree is -0.06MPa, the temperature is 68°C for 8 hours, and the modified rubber is dried at 50°C for 4 hours. (10) The modified rubber and styrene-butadiene rubber were respectively put into an open mill and plasticized at 55° C. for 7 min. The plasticized modified rubber and styrene-butadiene rubber were then mixed in a mass ratio of 30:12.

5. After mixing at 55° C. for 12 min, phenolic resin filler, stearic acid and antioxidant 4010 were added in a mass ratio of 14:1.5:0.75 (the mass ratio of the modified rubber to the phenolic resin filler was 30:14). The temperature was raised to 75° C. and mixed for 12 min. Then, sulfur and accelerator M were added in a mass ratio of 2:1.5 (the mass ratio of the modified rubber to sulfur was 30:2). After vulcanization at 150° C. for 9 min, the anti-skid and anti-penetration sole material was obtained by molding.