Environmentally friendly sponge and its preparation method and application in insoles
By using environmentally friendly low-emission raw materials and nano calcium carbonate or modified plant fibers, sponges with high tensile strength and low compression deformation are prepared, which solves the problem of difficult degradation of PU foamed sponges and improves environmental protection and mechanical properties. Suitable for insole applications.
Patent Information
- Application Number
- CN202410008817.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-04
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-01-04
AI Technical Summary
PU foam sponge insoles are difficult to degrade or recycle after being discarded, resulting in environmental pressure and affecting its marketing promotion.
Prepare sponges with environmentally friendly low-emission raw materials, including thermoplastic polyurethane, nano calcium carbonate or modified plant fibers as fill aggregates. The tensile strength, elongation of break and reduce compression of the sponge by treating foaming agents and functional additives. Deformation.
It significantly improves the mechanical properties of the sponge, reduces production pollution emissions, enhances environmental protection, and provides better support and durability when used in insoles.
Smart Images

Figure BDA0004648545630000091 
Figure BDA0004648545630000101 
Figure BDA0004648545630000102
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sponge insole manufacturing, and in particular to an environmentally friendly sponge and a preparation method thereof and application in an insole. Background Art
[0002] As a traditional Chinese product, insoles have a history of thousands of years. In modern society, with the advancement of science and technology, insoles, a product closely related to life, have gotten rid of a single function and have functions that are more in line with people's lives. For example, heating function and health care function can be added to insoles. As the functions of insoles increase, the research on the preparation materials of insoles is becoming increasingly in-depth.
[0003] At present, the main materials of insoles on the market are EVA, textiles, natural or artificial leather, PU foam sponge, silicone, etc. Among them, although the insoles made of EVA material are relatively soft and light, and have good comfort, their supporting capacity is insufficient and they are prone to deformation. PU foam sponge has good air permeability and moisture permeability, and adding some skeleton auxiliary materials to it can improve the supporting performance of PU foam sponge. Therefore, PU foam sponge has gradually become the main material of insoles.
[0004] However, with the widespread use of PU foam sponge insoles, and the insoles themselves are consumables, when PU foam sponge insoles are discarded, they are difficult to degrade or recycle, thus causing great pressure on the environment. This also affects the further promotion of PU foam sponge insoles in the market. Based on this, there is an urgent need to provide a solution to this problem. Summary of the invention
[0005] The purpose of the present invention is to provide an environmentally friendly sponge and a preparation method and application thereof. By using environmentally friendly and low-emission raw materials to prepare the sponge, the pollution emissions in the sponge production process can be reduced, which is more green and environmentally friendly, and the tensile strength and elongation at break of the environmentally friendly sponge can be improved, and the compression deformation can be reduced.
[0006] In a first aspect, the present invention provides an environmentally friendly sponge, which comprises, by weight, 100 parts of thermoplastic polyurethane, 5-10 parts of filling aggregate, 1-2 parts of foaming agent, 1-2 parts of anti-aging agent and 1-2 parts of functional additive; the filling aggregate comprises at least one of modified or unmodified nano calcium carbonate and modified or unmodified plant fiber, and the particle size of the filling aggregate is 100-150nm.
[0007] The environmentally friendly sponge provided by the present invention is prepared by using environmentally friendly low-emission raw materials, which can reduce pollution emissions in the sponge production process and is more environmentally friendly; at the same time, the filling aggregate is used as the sponge raw material, which can be dispersed in the molded sponge and form a skeleton network in the sponge, and is adsorbed and cross-linked with the sponge monomer. The filling aggregate is made into a nano-scale material, which can increase the specific surface area of the filling aggregate, thereby improving the adsorption and cross-linking ability, and can significantly enhance the tensile strength and elongation at break of the sponge, and reduce the compression deformation of the sponge; the foaming agent can foam the thermoplastic polyurethane, thereby increasing the porosity of the sponge, and cooperate with the filling aggregate to improve the distribution uniformity of the filling aggregate in the sponge.
[0008] Optionally, when the filling aggregate comprises modified nano-calcium carbonate, the preparation method of the modified nano-calcium carbonate comprises the following steps:
[0009] The nano calcium carbonate is dispersed in deionized water to prepare a calcium carbonate dispersion, ferric chloride hexahydrate is dissolved in the calcium carbonate dispersion and stirred and dispersed, sodium borohydride is added and stirred and dissolved, and then the mixture is kept warm at 40-45° C. and stirred for 6-7 hours, and then the solid is filtered out;
[0010] The solid was rinsed with anhydrous ethanol and resuspended with deionized water, and dodecyl dimethylamine oxide and hexadecyl dimethyl ammonium chloride were added and stirred to dissolve, and then the mixture was kept warm at 40-45° C. and stirred for 1-2 hours, and then filtered, ball-milled and sieved to obtain modified nano-calcium carbonate with a particle size of 100-150 nm.
[0011] By modifying the nano-calcium carbonate, the self-adsorption capacity of the nano-calcium carbonate can be improved, thereby improving the binding capacity of the nano-calcium carbonate with the sponge monomer, so that when the modified nano-calcium carbonate is dispersed in the sponge, it can form a filling network with a more stable morphology, thereby improving the mechanical properties of the sponge and reducing compression deformation; and in the process of modifying the nano-calcium carbonate, the iron ions are dispersed with the nano-calcium carbonate, and the iron ions are reduced to zero-valent iron using sodium borohydride. When the zero-valent iron is combined with the nano-calcium carbonate, the adsorption capacity of the nano-calcium carbonate can be significantly improved; after the surface of the nano-calcium carbonate is activated using dodecyl dimethyl amine oxide and hexadecyl dimethyl ammonium chloride, the binding capacity of the nano-calcium carbonate with the zero-valent iron can be improved.
[0012] Optionally, after the ferric chloride hexahydrate is dissolved in the calcium carbonate dispersion, the molar ratio of iron ions to calcium ions in the mixed solution is 1.2-1.5%. When the ferric chloride hexahydrate and the nano-calcium carbonate are mixed in such a ratio, when the iron ions are reduced to zero-valent iron, the iron ions can be more evenly dispersed in the nano-calcium carbonate, and when the sponge is prepared, the nano-calcium carbonate and iron will not be separated, thereby improving the overall structural stability of the modified nano-calcium carbonate.
[0013] Optionally, after sodium borohydride is added and stirred and dissolved, the molar ratio of sodium ions to iron ions in the mixed solution is 160-180%. By adding an appropriate amount of sodium borohydride, the iron ions dispersed in the mixed solution can be reduced, and the combination between sodium borohydride and nano-calcium carbonate is reduced, thereby reducing the content of sodium borohydride doped in the sponge raw material.
[0014] Optionally, when dodecyl dimethylamine oxide and hexadecyl dimethyl ammonium chloride are added and stirred to dissolve, the mass ratio of dodecyl dimethoxyamine oxide to hexadecyl dimethyl ammonium chloride is 1: 1. When dodecyl dimethoxyamine oxide and hexadecyl dimethyl ammonium chloride are compounded and used in a specific mass ratio, the activation ability of the surface of nano-calcium carbonate can be improved, thereby improving the binding ability of nano-calcium carbonate with iron.
[0015] Optionally, the mass ratio of the dodecyl dimethoxyamine oxide to the solid is 0.5-1%. In fact, when the mass ratio of dodecyl dimethoxyamine oxide, hexadecyl dimethyl ammonium chloride and the solid reaches this ratio, it can not only activate the surface of nano calcium carbonate well, but also improve the economy in the sponge preparation process.
[0016] Optionally, when the filling aggregate comprises modified plant fiber, the method for preparing the modified plant fiber comprises the following steps:
[0017] The plant fiber is soaked in a saturated solution of sodium hydroxide for 2-3 hours, then washed, dried, crushed and sieved, and 100-150nm powder is sieved out as the pre-treated fiber;
[0018] The pre-treated fiber is immersed in a mixture of cashew nut shell oil and polyethylene, immersed at 180-190° C. for 5-10 minutes, filtered and dried, and thus the modified plant fiber is obtained.
[0019] The skeleton effect of the plant fiber in the sponge can be improved by modifying the plant fiber, and when modifying the plant fiber, the plant fiber is immersed in a saturated solution of sodium hydroxide in advance for alkaline treatment, which can dissolve hemicellulose and pectin in the plant fiber and improve the surface roughness of the plant fiber, so that the specific surface area of the pre-treated fiber obtained by grinding and crushing the plant fiber can be significantly increased, and after the pre-treated fiber forms a fiber network in the sponge, it has good tensile strength and impact resistance; when the pre-treated fiber is immersed in a mixed solution of cashew nut shell oil and polyethylene at high temperature, the cashew nut shell oil and polyethylene are infiltrated into the pre-treated fiber, which can improve the cross-linking performance of the modified plant fiber and the sponge monomer, thereby improving the bonding performance of the sponge and the modified plant fiber.
[0020] Optionally, the plant fiber includes at least one of jute fiber, flax fiber and bamboo fiber. In fact, jute fiber, flax fiber and bamboo fiber are common fiber materials, thereby reducing the industrial cost of sponge preparation, and jute fiber, flax fiber and bamboo fiber are environmentally friendly materials. When the sponge is degraded, the plant fiber can also be recycled and is not easy to cause pollution.
[0021] Optionally, when the pre-treated fiber is immersed in a mixture of cashew nut shell oil and polyethylene, the mass ratio of cashew nut shell oil to the polyethylene in the mixture is 10-20, and the mass ratio of the cashew nut shell oil to the pre-treated fiber is 10:1.
[0022] Optionally, when the filling aggregate includes modified nano-calcium carbonate and modified plant fiber, the mass ratio of the modified nano-calcium carbonate to the modified plant fiber is 1: 1. In fact, when the modified nano-calcium carbonate and the modified plant fiber are mixed in a specific mass ratio, a composite skeleton network can be formed in the sponge, thereby improving the mechanical properties of the sponge and reducing the compression deformation of the sponge.
[0023] In a second aspect, the present invention also provides a method for preparing an environmentally friendly sponge, comprising the following steps:
[0024] The thermoplastic polyurethane and the filler aggregate are uniformly dispersed at 120-150° C., and stirred and kept warm for 1-2 hours in an environment of 0.1-0.2 standard atmospheric pressure to obtain a first mixture;
[0025] After adding the anti-aging agent and the functional additive to the first mixed material and stirring and mixing, adding the foaming agent under normal pressure and performing foaming and vulcanization in a mixer to obtain a sponge foaming liquid;
[0026] The environmentally friendly sponge is prepared by cold-pressing the sponge foaming liquid to shape it.
[0027] The preparation method of the environmentally friendly sponge provided by the present invention can prepare the environmentally friendly sponge by adopting simple mixing steps, thereby reducing the VOC gas generated in the sponge production process.
[0028] Optionally, when adding the anti-aging agent and the functional additive to the first mixed material and stirring and mixing, the rotation speed is controlled to be 100-120 rpm and the temperature is controlled to be 150-170°C.
[0029] In a third aspect, the present invention further provides an application of an environmentally friendly sponge in an insole, comprising the following steps:
[0030] The thermoplastic polyurethane and the filler aggregate are uniformly dispersed at 120-150° C., and stirred and kept warm for 1-2 hours in an environment of 0.1-0.2 standard atmospheric pressure to obtain a first mixture;
[0031] After adding the anti-aging agent and the functional additive to the first mixed material and stirring and mixing, adding the foaming agent under normal pressure and performing foaming and vulcanization in a mixer to obtain a sponge foaming liquid;
[0032] The sponge foaming liquid is injected into the insole mold for cold pressing and shaping to obtain the sponge insole. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be understood by people with general skills in the field to which the present invention belongs. "Including" and similar words used in this article mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.
[0034] The embodiment of the present invention provides an environmentally friendly sponge, which includes 100 parts of thermoplastic polyurethane, 5-10 parts of filling aggregate, 1-2 parts of foaming agent, 1-2 parts of anti-aging agent and 1-2 parts of functional additives in parts by weight.
[0035] In fact, thermoplastic polyurethane is an environmentally friendly sponge raw material with excellent comprehensive properties such as high strength, high toughness, wear resistance, oil resistance, aging resistance, etc., and it has good processing performance. After adding a variety of functional additives to thermoplastic polyurethane elastomers, the overall performance or monomer performance of thermoplastic polyurethane can be improved, and it has a wide range of applications.
[0036] Specifically, the thermoplastic polyurethane in the environmentally friendly sponge can be polyester polyurethane, and a conventional commercial product can be selected, specifically one of 385SX, 192X, 390X, 345X, 359X, 365X, 372X of the Desmopan series, 258, 245, 250, 255, 260, 270 of the TEXIN series, and US75AU, US80AU, U85AU, U-90AU, U-95AU, and U-98AU of the UTECHHLLAN series.
[0037] Specifically, the foaming agent can be any one of an inorganic foaming agent and an organic foaming agent. Specifically, when the foaming agent is an inorganic foaming agent, it can be carbon dioxide, nitrogen and other inert gases. When the foaming agent is an organic foaming agent, it can be a C4-C10 alkane, such as butane, pentane, heptane and octane and their isomers.
[0038] Specifically, the anti-aging agent can be a conventional commercial product or a separately synthesized compound, for example, it can be a UV stabilizer, a UV shielding agent, an antioxidant, specifically antioxidant 1010, UV absorber UV-1, 2,4-dihydroxybenzophenone, 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid.
[0039] Specifically, the functional additives can be additives commonly used in the art, such as dyes, plasticizers, and dispersants. For example, the functional additives can be dye masterbatches. By using dye masterbatches, the sponges can be dyed, so that the environmentally friendly sponges have a variety of colors, thereby improving the performance and aesthetics of the environmentally friendly sponges. For example, the functional additives can also be plasticizers. By adding plasticizers to the sponges, the secondary bonds between the sponge monomers can be reduced, the mobility of the molecular bonds can be increased, and the crystallinity of the sponge monomers can be reduced, thereby improving the plasticity of the sponge, which is beneficial for shaping the environmentally friendly sponges.
[0040] Specifically, the filling aggregate includes at least one of unmodified nano calcium carbonate, modified nano calcium titanate, unmodified plant fiber and modified plant fiber. By adding the filling aggregate into the sponge, when the filling aggregate is dispersed in the sponge, the filling aggregate can form a dense and uniform skeleton network, and adsorb and cross-link with the sponge monomer, thereby improving the overall mechanical properties of the sponge, and can also support the sponge and reduce the compression deformation of the sponge.
[0041] In fact, the particle size of the filling aggregate is 100-150nm. By using filling aggregate within this particle size range, it is easier to disperse evenly in the sponge raw material. At the same time, the filling aggregate can have a larger specific surface area, so that it can better adsorb the sponge monomer, avoid the precipitation of the filling aggregate from the sponge, and further improve the overall mechanical properties of the sponge.
[0042] In some embodiments, when the filling aggregate includes modified nano-calcium carbonate, the preparation method of the modified nano-calcium carbonate includes the following steps:
[0043] The nano calcium carbonate is dispersed in deionized water to prepare a calcium carbonate dispersion, ferric chloride hexahydrate is dissolved in the calcium carbonate dispersion and stirred and dispersed, sodium borohydride is added and stirred and dissolved, and then the mixture is kept warm at 40-45° C. and stirred for 6-7 hours, and then the solid is filtered out;
[0044] The solid was rinsed with anhydrous ethanol and resuspended with deionized water, and dodecyl dimethylamine oxide and hexadecyl dimethyl ammonium chloride were added and stirred to dissolve, and then the mixture was kept warm at 40-45° C. and stirred for 1-2 hours, and then filtered, ball-milled and sieved to obtain modified nano-calcium carbonate with a particle size of 100-150 nm.
[0045] Specifically, after dispersing nano-calcium carbonate in deionized water to prepare a calcium carbonate dispersion, the mass fraction of the nano-calcium carbonate in the calcium carbonate dispersion is 10-15%. When dispersed at this mass fraction, the dispersion uniformity of the nano-calcium carbonate in the calcium carbonate dispersion can be improved, which is beneficial to the surface doping and surface modification of the nano-calcium carbonate in the subsequent process.
[0046] Specifically, after dissolving ferric chloride hexahydrate in a calcium carbonate dispersion and stirring and dispersing, the molar ratio of iron ions to calcium ions in the mixed solution is 1.2-1.5%. Mixing ferric chloride hexahydrate and nano-calcium carbonate at this molar ratio is beneficial to improving the dispersion uniformity of iron ions in the mixed solution, and is also beneficial to the mixing of iron ions and calcium ions, thereby facilitating the binding relationship between zero-valent iron and calcium ions after the subsequent reduction of iron ions.
[0047] Specifically, when sodium borohydride is added and stirred and dissolved, the sodium borohydride can be added to the dispersion after the ferric chloride and nano-calcium carbonate are mixed in the form of a solution, a compound, or a single substance. In fact, after the sodium borohydride is added and stirred and dissolved, the molar ratio of sodium ions to iron ions in the mixed solution is 160-180%. By using sodium borohydride with this molar ratio, it is more conducive to reducing iron ions to zero-valent iron, and it can also reduce the mixing of sodium borohydride and calcium ions, thereby reducing the amount of sodium borohydride entering the sponge.
[0048] Specifically, when dodecyl dimethyl amine oxide and hexadecyl dimethyl ammonium chloride are added and stirred to dissolve, the mass ratio of dodecyl dimethoxy amine oxide to hexadecyl dimethyl ammonium chloride is 1:1; specifically, the mass ratio of dodecyl dimethoxy amine oxide to the solid matter in the mixed solution is 0.5-1%.
[0049] In some embodiments, when the filler aggregate includes modified plant fibers, the method for preparing the modified plant fibers includes the following steps:
[0050] The plant fiber is soaked in a saturated solution of sodium hydroxide for 2-3 hours, then washed, dried, crushed and sieved, and 100-150nm powder is sieved out as the pre-treated fiber;
[0051] The pre-treated fiber is immersed in a mixture of cashew nut shell oil and polyethylene, immersed at 180-190° C. for 5-10 minutes, filtered and dried, and thus the modified plant fiber is obtained.
[0052] Specifically, the plant fiber includes at least one of jute fiber, flax fiber and bamboo fiber; when the pre-treated fiber is immersed in a mixture of cashew nut shell oil and polyethylene, the mass ratio of cashew nut shell oil to polyethylene in the mixture is 10-20, and the mass ratio of cashew nut shell oil to pre-treated fiber is 10:1, and specifically, the molecular weight of polyethylene can be 10000-15000. In fact, when the filling aggregate includes modified nano calcium carbonate and modified plant fiber, the mass ratio of modified nano calcium carbonate to modified plant fiber is 1:1.
[0053] In fact, an embodiment of the present invention also provides a method for preparing any of the above-mentioned environmentally friendly sponges, comprising the following steps:
[0054] The thermoplastic polyurethane and the filler aggregate are uniformly dispersed at 120-150° C., and stirred and kept warm for 1-2 hours in an environment of 0.1-0.2 standard atmospheric pressure to obtain a first mixture;
[0055] After adding the anti-aging agent and the functional additive to the first mixed material and stirring and mixing, adding the foaming agent under normal pressure and performing foaming and vulcanization in a mixer to obtain a sponge foaming liquid; specifically, the speed is controlled to be 100-120rpm and the temperature is 150-170°C;
[0056] The environmentally friendly sponge is prepared by cold-pressing the sponge foaming liquid to shape it.
[0057] Specifically, when preparing the environmentally friendly sponge, the sponge foaming liquid can be cold-pressed and shaped in an insole mold to obtain the environmentally friendly sponge insole.
[0058] Examples 1-5
[0059] The present embodiments 1-5 provide an environmentally friendly sponge, respectively, and the raw materials and weight portions thereof are shown in the following Table 1:
[0060] Table 1
[0061]
[0062]
[0063] Examples 6-10
[0064] Embodiments 6-10 provide an environmentally friendly sponge, respectively, and the raw materials and weight portions thereof are shown in Table 2 below:
[0065] Table 2
[0066]
[0067] Among them, the thermoplastic polyurethane used in Examples 1-10 is specifically TEXI N-258, the plant fiber used is specifically jute fiber, the foaming agent used is specifically butane, the anti-aging agent used is specifically a mixture of antioxidant 1010 and ultraviolet absorber UV-1 in a mass ratio of 1:1, and the functional additive used is specifically a plasticizer (di(2-ethylhexyl) phthalate).
[0068] Specifically, the preparation method of the modified nano calcium carbonate used in Examples 1-10 comprises the following steps:
[0069] Dispersing nano calcium carbonate in deionized water to prepare a carbonic anhydride dispersion containing 15% of the mass fraction of nano calcium carbonate;
[0070] Dissolving ferric chloride hexahydrate in a calcium carbonate dispersion and stirring to disperse the mixture, wherein the amount of ferric chloride hexahydrate added is such that the molar ratio of iron ions to calcium ions in the mixture is 1.5%;
[0071] Sodium borohydride was then added and stirred to dissolve, and then mechanically stirred at 45° C. and 200 rpm for 7 hours, and then the solid was centrifuged and filtered out; wherein the amount of sodium borohydride added was such that the molar ratio of sodium ions to iron ions in the mixed solution was 1.7;
[0072] The solid was rinsed with anhydrous ethanol and then resuspended with deionized water, and dodecyl dimethylamine oxide and hexadecyl dimethyl ammonium chloride were added and stirred to dissolve, and then the mixture was kept warm at 45°C and mechanically stirred at 200 rpm for 2 hours, and then filtered, ball-milled and sieved to obtain modified nano-calcium carbonate with a particle size of 100-150 nm; wherein the mass ratio of dodecyl dimethoxyamine oxide to the solid in the mixed solution was 0.01.
[0073] Specifically, the method for preparing the modified plant fiber used in Examples 1-10 comprises the following steps:
[0074] The jute fiber is soaked in a saturated solution of sodium hydroxide for 3 hours, washed, dried, crushed and sieved, and the powder of 100-150 nm is the pre-treated fiber;
[0075] The pre-treated fiber is immersed in a mixture of cashew nut shell oil and polyethylene, and then filtered and dried after soaking at 180-190° C. for 5-10 minutes to obtain a modified plant fiber; wherein the mass ratio of cashew nut shell oil to polyethylene in the mixture is 10-20, and the mass ratio of cashew nut shell oil to pre-treated fiber is 10:1.
[0076] The preparation method of the environmentally friendly sponge in the present embodiment 1-10 comprises the following steps:
[0077] The thermoplastic polyurethane and the filler aggregate are uniformly dispersed at 150° C., and stirred and kept warm for 1.5 hours in an environment of 0.2 standard atmospheric pressure to obtain a first mixture;
[0078] After adding the anti-aging agent and the functional additive to the first mixture and stirring and mixing, the foaming agent is added under normal pressure and foaming and vulcanization are carried out in a mixer to obtain a sponge foaming liquid; specifically, the speed is controlled to be 120rpm and the temperature is 160°C; the sponge foaming liquid is cold-pressed and formed to obtain an environmentally friendly sponge.
[0079] Comparative Example 1
[0080] This comparative example 1 provides an environmentally friendly sponge, which is different from Example 8 in that no filler aggregate is added to the raw materials of the environmentally friendly sponge in comparative example 1.
[0081] Performance Testing
[0082] The environmentally friendly sponges prepared in Examples 1-10 and Comparative Example 1 were tested, and the specific test indicators and test methods are as follows, and the results are recorded in Table 3:
[0083] Apparent density: Based on GB / T 6343-2009 Determination of apparent density of foam plastics and rubber, unit is kg / m 3 ;
[0084] Rebound rate: Based on GB / T 10652-2001 Determination of elasticity of polymer porous elastic materials, unit is %;
[0085] Compression deformation: Based on GB / T 10653-2001 Determination of compression permanent deformation of polymer porous elastic materials, unit is mm;
[0086] Tensile strength: Based on GB / T 6344-2008 Determination of tensile strength and elongation at break of flexible foam materials, using an electronic tensile testing machine, measured at a moving rate of 500±50mm / min, the unit is kPa;
[0087] Elongation at break: Based on GB / T 6344-2008 Determination of tensile strength and elongation at break of flexible foam materials, using an electronic tensile testing machine, with a moving rate of 500±50mm / min, the unit is %;
[0088] Degradation rate: The maximum biodegradability is determined based on GB / T 19277.1-2011 Determination of the ultimate aerobic biodegradability of materials under controlled composting by measuring the released carbon dioxide Part 1: General method, and the unit is %.
[0089] Table 3
[0090]
[0091]
[0092] It can be seen from Examples 1-10 and Comparative Example 1 that the environmentally friendly sponge provided by the present invention has a better degradation rate. Although the surface density of the sponge has increased due to the addition of filler aggregates in Examples 1-10, it is still within the qualified range, and the overall rebound rate, compression deformation, tensile strength and elongation at break of the environmentally friendly sponge are greatly improved compared with Comparative Example 1.
[0093] From Examples 1-4, combined with Table 3, it can be seen that when a single filling aggregate is selected, the modified and unmodified nano-calcium carbonate has a good promoting effect on the overall rebound rate of the sponge and can also reduce the compression deformation of the sponge. From Examples 3 and 4, it can be seen that although the plant fiber is modified, the effect of the modified plant fiber on the rebound rate and compression deformation of the sponge is not particularly significant.
[0094] From Example 1, Example 3 and Example 5, and in combination with Table 3, it can be seen that when the filling aggregate is composited with unmodified nano-calcium carbonate and unmodified plant fiber, the total content of nano-calcium carbonate in the sponge decreases, which has some negative effects on the resilience of the sponge. This shows that if the filling aggregate is composited with unmodified nano-calcium carbonate and unmodified plant fiber, there is no synergistic effect.
[0095] From Examples 1-2 and 6, and in combination with Table 3, it can be seen that when unmodified nano-calcium carbonate and modified nano-calcium carbonate are used in combination as filling aggregates, the resilience of the sponge is promoted to some extent. This may be because the modified nano-calcium carbonate can be more easily combined with calcium carbonate, thereby forming a more robust network structure in the sponge, thereby improving the resilience of the sponge.
[0096] From Example 1, Example 4 and Example 7, combined with Table 3, it can be seen that when the filling aggregate is composited with unmodified nano-calcium carbonate and modified plant fiber, the resilience of the sponge decreases compared to Example 1, which indicates that the unmodified nano-calcium carbonate is difficult to be evenly mixed with the modified plant fiber to form a stable skeleton network, resulting in a slight decrease in the resilience of the sponge.
[0097] It can be seen from Example 2, Example 4 and Example 8, combined with Table 3, that when the modified nano-calcium carbonate and the modified plant fiber are used as the filling aggregate in a mass ratio of 1:1, the resilience of the sponge can be significantly improved.
[0098] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.
Claims
1. An environmentally friendly sponge, characterized in that: The invention comprises, by weight, 100 parts of thermoplastic polyurethane, 5-10 parts of filling aggregate, 1-2 parts of foaming agent, 1-2 parts of anti-aging agent and 1-2 parts of functional additive; the filling aggregate is composed of modified nano-calcium carbonate and modified plant fiber, and the particle size of the filling aggregate is 100-150nm; the mass ratio of the modified nano-calcium carbonate to the modified plant fiber is 1:1; The preparation method of the environmentally friendly sponge comprises the following steps: uniformly dispersing thermoplastic polyurethane and filler aggregate at 120-150° C., stirring and keeping warm for 1-2 hours in an environment of 0.1-0.2 standard atmospheric pressure to obtain a first mixed material; adding an anti-aging agent and a functional auxiliary agent to the first mixed material, stirring and mixing, adding a foaming agent under normal pressure, and performing foaming and vulcanization in a mixer to obtain a sponge foaming liquid; cold-pressing and shaping the sponge foaming liquid to obtain an environmentally friendly sponge; The preparation method of the modified nano calcium carbonate comprises the following steps: dispersing nano calcium carbonate in deionized water to prepare a calcium carbonate dispersion, dissolving ferric chloride hexahydrate in the calcium carbonate dispersion, stirring and dispersing, adding sodium borohydride, stirring and dissolving, keeping warm at 40-45° C. and stirring for 6-7 hours, and then filtering out the solid; washing the solid with anhydrous ethanol, resuspending it with deionized water, adding dodecyl dimethylamine oxide and hexadecyl dimethyl ammonium chloride, stirring and dissolving, keeping warm at 40-45° C. and stirring for 1-2 hours, and then resuspending it with deionized water; Filtering, ball milling and sieving to obtain modified nano calcium carbonate with a particle size of 100-150nm; after dissolving ferric chloride hexahydrate in calcium carbonate dispersion, the molar ratio of iron ions to calcium ions in the mixed solution is 1.2-1.5%; after adding sodium borohydride and stirring to dissolve, the molar ratio of sodium ions to iron ions in the mixed solution is 160-180%; the mass ratio of dodecyl dimethoxy amine oxide to hexadecyl dimethyl ammonium chloride is 1:1, and the mass ratio of dodecyl dimethoxy amine oxide to the solid is 0.5-1%; The preparation method of the modified plant fiber comprises the following steps: soaking the plant fiber in a saturated solution of sodium hydroxide for 2-3 hours, washing, drying, crushing and screening, and screening out 100-150nm powder as pre-treated fiber; immersing the pre-treated fiber in a mixed solution of cashew nut shell oil and polyethylene, soaking at 180-190°C for 5-10 minutes, filtering and drying, and obtaining the modified plant fiber; wherein the plant fiber is jute fiber; the mass ratio of cashew nut shell oil to the polyethylene in the mixed solution is 10-20, and the mass ratio of the cashew nut shell oil to the pre-treated fiber is 10:
1.
2. The environmentally friendly sponge according to claim 1, characterized in that: When adding the anti-aging agent and the functional additive to the first mixed material and stirring and mixing, the rotation speed is controlled to be 100-120rpm and the temperature is controlled to be 150-170°C.
3. An application of the environmentally friendly sponge as claimed in any one of claims 1 to 2 in insoles, characterized in that: The following steps are involved: The thermoplastic polyurethane and the filler aggregate are uniformly dispersed at 120-150° C., and stirred and kept warm for 1-2 hours in an environment of 0.1-0.2 standard atmospheric pressure to obtain a first mixture; After adding the anti-aging agent and the functional additive to the first mixed material and stirring and mixing, adding the foaming agent under normal pressure and performing foaming and vulcanization in a mixer to obtain a sponge foaming liquid; The sponge foaming liquid is injected into the insole mold for cold pressing and shaping to obtain the sponge insole.