A mixed decolorizing agent
By combining modified dicyandiamide formaldehyde resin polymer and additives, a mixed decolorizing agent for liquid crystal display wastewater treatment was prepared, which solved the problem of unsatisfactory chromaticity and organic matter removal effects in the existing technology, and achieved Efficient wastewater treatment, especially in applications in the LCD manufacturing industry, significantly improves the purification effect of wastewater.
Patent Information
- Application Number
- CN202410103475.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2023-10-09
- Filing Date
- 2024-01-25
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-01-25
AI Technical Summary
The color film wastewater from the LCD industry has high chroma and high organic matter content. The existing treatment process has unsatisfactory removal effect on chroma, and the physical and chemical method decolorizes quickly but has low organic matter removal effect, which leads to the need to develop efficient decolorizing agents.
Modified dicyandiamide formaldehyde resin polymer is compounded with other additives to prepare a mixed decolorizing agent, including polydimethyldiallylammonium chloride, polymerized ferric sulfate, polymerized aluminum sulfate, diatomaceous earth, activated carbon and Aluminum sulfate, through the etherification reaction of modified dicyandiamide formaldehyde resin polymer and 4-hydroxy-3-nitrobenzyl alcohol and the modification treatment of diatomaceous earth, has good decolorization effect, COD removal effect and ammonia nitrogen removal effect. mixed decolorizing agent.
It achieves the fundamental removal of multiple pollutants in wastewater, improves the decolorization performance and rate, has strong flocculation effect and stability, and significantly improves the removal rate of chroma, COD and ammonia nitrogen.
Smart Images

Figure CN117843901B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water treatment, and in particular relates to a mixed decolorizing agent. Background Art
[0002] Color film wastewater in the LCD industry generally contains pigments, alkali-soluble resins (alkali-soluble polymers), photopolymer monomer components, and color additives such as photoinitiators, dispersants, emulsifiers, and solvents. At present, the color film (CF) of LCDs is mainly made of pigment dispersion materials. The manufacturing methods include photolithography, printing, electroprecipitation, inkjet coating, etc. Among them, pigment dispersion photolithography is the most widely used method. Pigment particles with a diameter of less than 0.7μm are dispersed in photoresist, and dispersants are used to disperse the pigment particles and prevent the particles from agglomerating. First, Cr film is plated on a 0.7mm thick glass substrate, and then the black matrix (BM) pattern is obtained by photolithography. Next, red pigment is applied and photoresist is dispersed. After exposure, development, etching, stripping and other photolithography processes, a red film is obtained. Repeat the same photolithography process to obtain green and blue film patterns respectively.
[0003] The wastewater produced by this production line has the characteristics of high chromaticity, high organic content, containing pollutants such as pigment colloids and additives, strong alkalinity, and large fluctuations in water quality. At present, most of the treatment processes used are mainly biochemical treatment and supplemented by physical and chemical treatment. The biological treatment method has good effect in removing organic matter and low cost, but it is not ideal for removing chromaticity; the physical and chemical method is fast and efficient in decolorization, but the removal effect of organic matter is low. Therefore, it is of great significance to develop an efficient decolorizer. Summary of the invention
[0004] The object of the present invention is to provide a mixed decolorizing agent, which has good decolorizing effect, COD removal effect and ammonia nitrogen removal effect.
[0005] The technical solution adopted by the present invention to achieve the above-mentioned purpose is:
[0006] A modified dicyandiamide formaldehyde resin polymer comprises a dicyandiamide formaldehyde resin polymer and a surface modification group thereof; the surface modification group is selected from at least one of a nitro group and an aromatic ring group.
[0007] The invention also discloses a method for preparing a modified dicyandiamide formaldehyde resin polymer, comprising: carrying out an etherification reaction between 4-hydroxy-3-nitrobenzyl alcohol and the dicyandiamide formaldehyde resin polymer to prepare the modified dicyandiamide formaldehyde resin polymer.
[0008] The invention provides a method for preparing a modified dicyandiamide formaldehyde resin polymer. The modified dicyandiamide formaldehyde resin polymer is etherified with 4-hydroxy-3-nitrobenzyl alcohol. The obtained modified dicyandiamide formaldehyde resin polymer is used for preparing a mixed decolorizing agent, so that the mixed decolorizing agent has good decolorizing effect, COD removal effect and ammonia nitrogen removal effect.
[0009] Specifically, the preparation method of the modified dicyandiamide formaldehyde resin polymer comprises the following steps:
[0010] The dicyandiamide is added to distilled water (the mass volume ratio of the two is: 1g:30-45mL), the pH is adjusted to 9-10 at 75-90°C, and then a formaldehyde aqueous solution with a concentration of 30-35wt% is slowly added, and the reaction is carried out at a constant temperature for 1.5-3h, and then the pH is adjusted to 4.5-6, and ammonium chloride is added, and the reaction is carried out at 60-70°C for 1-2h, and distillation is carried out under reduced pressure to obtain a dicyandiamide formaldehyde resin polymer; 4-hydroxy-3-nitrobenzyl alcohol is stirred and melted at 100-105°C, and then the dicyandiamide formaldehyde resin polymer is added, the pH is adjusted to 1.8-2.5, and the reaction is carried out at a constant temperature for 1-1.5h, filtered, cooled to room temperature, and distilled water-acetone (the volume ratio of distilled water to acetone is 1:1.5-2.5) is added to precipitate for 3-5 times, and dried to obtain a modified dicyandiamide formaldehyde resin polymer.
[0011] In the present invention, the molar ratio of dicyandiamide to formaldehyde is 1:2.5-4; the molar ratio of dicyandiamide to ammonium chloride is 1:0.65-1.3.
[0012] In the present invention, the molar ratio of the dicyandiamide formaldehyde resin polymer to 4-hydroxy-3-nitrobenzyl alcohol is 1:3-4.
[0013] The invention also discloses the use of the modified dicyandiamide formaldehyde resin polymer prepared by the preparation method in preparing a decolorizing agent.
[0014] The invention also discloses the use of the modified dicyandiamide formaldehyde resin polymer prepared by the preparation method in the treatment of wastewater in the liquid crystal display manufacturing industry.
[0015] A mixed decolorizing agent comprises the modified dicyandiamide formaldehyde resin polymer.
[0016] For the present invention, the mixed decolorizing agent further comprises polydimethyldiallylammonium chloride, polyferric sulfate, polyaluminum sulfate, diatomaceous earth, activated carbon and aluminum sulfate.
[0017] The invention compounds a modified dicyandiamide formaldehyde resin polymer with other additives, and pollutants in wastewater are adsorbed, flocculated and precipitated by the modified dicyandiamide formaldehyde resin polymer and polydimethyldiallyl ammonium chloride, polyferric sulfate, polyaluminum sulfate, aluminum sulfate, diatomaceous earth and activated carbon, and multiple comprehensive effects are used in combination to improve the decolorization performance and decolorization rate, and can also fundamentally remove pollutants, and has the characteristics of good decolorization effect, strong flocculation effect, high stability and the like.
[0018] For the present invention, in the above-mentioned mixed decolorizing agent, by weight, the amount of modified dicyandiamide formaldehyde resin polymer is 20 to 50 parts, the amount of polydimethyldiallylammonium chloride is 1 to 5 parts, the amount of polyferric sulfate is 1 to 3 parts, the amount of polyaluminum sulfate is 1 to 3 parts, the amount of diatomaceous earth is 1 to 3 parts, the amount of activated carbon is 2 to 8 parts, and the amount of aluminum sulfate is 2 to 6 parts.
[0019] The invention also discloses the use of the mixed decolorizing agent in wastewater treatment.
[0020] In order to further improve the performance of the mixed decolorizing agent, the present invention further modifies the diatomaceous earth.
[0021] The invention also discloses a method for preparing modified diatomite, comprising: using gamma-glycidyloxypropyltrimethoxysilane to undergo condensation reaction with diatomite, then performing a ring-opening reaction, and then performing an esterification reaction with chlorinated p-carboxybenzenesulfonamide to obtain the modified diatomite.
[0022] Specifically, the preparation method of the modified diatomite comprises the following steps:
[0023] Step 1, add ethanol to diatomaceous earth (the mass volume ratio of diatomaceous earth to ethanol is: 1g:10-20mL), then slowly add γ-glycidyloxypropyltrimethoxysilane at 38-55°C, react at constant temperature for 3-7h, filter, wash with ethanol, and dry to obtain condensation-modified diatomaceous earth;
[0024] Step 2: Add distilled water, tetrahydrofuran and cobalt acetate tetrahydrate to the condensed modified diatomaceous earth, stir and mix at 0-5° C. for 20-30 hours, then naturally warm to room temperature, stand for 20-30 hours, filter, wash with ethanol 3-5 times, and dry to obtain open-ring diatomaceous earth;
[0025] Step 3: Add thionyl chloride to the open-ring diatomaceous earth, then add p-carboxybenzenesulfonamide, stir and mix evenly, react at 100-105° C. for 3.5-5 hours, wash with distilled water 3-5 times, and wash with methanol 3-5 times to obtain modified diatomaceous earth.
[0026] In the present invention, in the above step 1, the mass volume ratio of diatomaceous earth to γ-glycidyloxypropyltrimethoxysilane is: 1g:3-7mL.
[0027] For the present invention, the ethanol in the above step 1 is an ethanol aqueous solution with a concentration of 80wt%.
[0028] For the present invention, in the above step 2, the mass volume ratio of the condensation-modified diatomaceous earth to distilled water is: 1 g: 10-20 mL; the mass volume ratio of the condensation-modified diatomaceous earth to tetrahydrofuran is: 1 g: 0.15-0.25 mL; the mass ratio of the condensation-modified diatomaceous earth to cobalt acetate tetrahydrate is: 1: 0.005-0.01.
[0029] For the present invention, in the above step 3, the mass volume ratio of the opened diatomaceous earth to thionyl chloride is: 1 g: 40-60 mL; the mass ratio of the opened diatomaceous earth to p-carboxybenzenesulfonamide is: 1: 2.5-5.5.
[0030] The invention also discloses the use of the modified diatomaceous earth prepared by the preparation method in preparing a decolorizing agent.
[0031] The invention also discloses the use of the modified diatomaceous earth prepared by the preparation method in the treatment of wastewater in the liquid crystal display manufacturing industry.
[0032] The beneficial effects of the present invention include:
[0033] The invention provides a mixed decolorizing agent. The mixed decolorizing agent is prepared by mixing a dicyandiamide formaldehyde resin polymer modified by 4-hydroxy-3-nitrobenzyl alcohol with polydimethyldiallylammonium chloride, polyferric sulfate, polyaluminium sulfate, diatomaceous earth, activated carbon and aluminium sulfate. The prepared mixed decolorizing agent has good decolorizing effect, COD removal effect and ammonia nitrogen removal effect. In addition, the invention also adopts p-carboxybenzenesulfonamide to modify the diatomaceous earth. The prepared modified diatomaceous earth is used for preparing the mixed decolorizing agent, so that the mixed decolorizing agent has better decolorizing effect, COD removal effect and ammonia nitrogen removal effect.
[0034] Therefore, the present invention provides a mixed decolorizing agent, which has good decolorizing effect, COD removal effect and ammonia nitrogen removal effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The infrared spectra test results of the modified dicyandiamide formaldehyde resin polymer and the dicyandiamide formaldehyde resin polymer prepared in Example 1;
[0036] Figure 2 These are the test results of infrared spectra of the modified diatomite, ring-opened diatomite, condensation-modified diatomite and diatomite prepared in Example 5. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the present invention more clear, the technical solution of the present invention is further described in detail below in conjunction with specific implementation methods:
[0038] Embodiment 1:
[0039] A method for preparing a mixed decolorizing agent comprises: uniformly stirring and mixing a modified dicyandiamide formaldehyde resin polymer, polydimethyldiallyl ammonium chloride, polyferric sulfate, polyaluminum sulfate, diatomaceous earth, activated carbon and aluminum sulfate to obtain a mixed decolorizing agent. In the mixed decolorizing agent, the amount of the modified dicyandiamide formaldehyde resin polymer is 20 parts by weight, the amount of polydimethyldiallyl ammonium chloride is 1 part, the amount of polyferric sulfate is 1 part, the amount of polyaluminum sulfate is 1 part, the amount of diatomaceous earth is 1 part, the amount of activated carbon is 2 parts, and the amount of aluminum sulfate is 2 parts.
[0040] The preparation method of modified dicyandiamide formaldehyde resin polymer comprises the following steps:
[0041] Dicyandiamide was added to distilled water (the mass volume ratio of the two was 1 g:30 mL), the pH was adjusted to 9 at 75° C., then a 30 wt % formaldehyde aqueous solution was slowly added, the reaction was carried out at a constant temperature for 3 h, then the pH was adjusted to 4.5, ammonium chloride was added, the reaction was carried out at 60° C. for 2 h, and distillation was performed under reduced pressure to obtain a dicyandiamide formaldehyde resin polymer; 4-hydroxy-3-nitrobenzyl alcohol was stirred and melted at 100° C., and then the dicyandiamide formaldehyde resin polymer was added, the pH was adjusted to 2, the reaction was carried out at a constant temperature for 1.5 h, filtered, cooled to room temperature, distilled water-acetone (the volume ratio of distilled water to acetone was 1:1.5) was added, precipitated 3 times, and dried to obtain a modified dicyandiamide formaldehyde resin polymer; wherein the molar ratio of dicyandiamide to formaldehyde was 1:2.5; the molar ratio of dicyandiamide to ammonium chloride was 1:0.65; and the molar ratio of dicyandiamide formaldehyde resin polymer to 4-hydroxy-3-nitrobenzyl alcohol was 1:3.
[0042] Embodiment 2:
[0043] The difference between a preparation method of a mixed decolorizing agent and Example 1 is that in the mixed decolorizing agent, by weight, the amount of modified dicyandiamide formaldehyde resin polymer is 50 parts, the amount of polydimethyldiallylammonium chloride is 5 parts, the amount of polyferric sulfate is 3 parts, the amount of polyaluminum sulfate is 3 parts, the amount of diatomaceous earth is 3 parts, the amount of activated carbon is 8 parts, and the amount of aluminum sulfate is 6 parts.
[0044] The differences between the preparation method of the modified dicyandiamide formaldehyde resin polymer and Example 1 are as follows: the molar ratio of dicyandiamide to formaldehyde is 1:4; the molar ratio of dicyandiamide to ammonium chloride is 1:1.3; and the molar ratio of dicyandiamide formaldehyde resin polymer to 4-hydroxy-3-nitrobenzyl alcohol is 1:4.
[0045] Embodiment 3:
[0046] The difference between a preparation method of a mixed decolorizing agent and Example 1 is that in the mixed decolorizing agent, by weight, the amount of modified dicyandiamide formaldehyde resin polymer is 30 parts, the amount of polydimethyldiallylammonium chloride is 3 parts, the amount of polyferric sulfate is 2 parts, the amount of polyaluminum sulfate is 2 parts, the amount of diatomaceous earth is 2.5 parts, the amount of activated carbon is 5 parts, and the amount of aluminum sulfate is 4 parts.
[0047] The differences between the preparation method of the modified dicyandiamide formaldehyde resin polymer and Example 1 are as follows: the molar ratio of dicyandiamide to formaldehyde is 1:3; the molar ratio of dicyandiamide to ammonium chloride is 1:1; and the molar ratio of dicyandiamide formaldehyde resin polymer to 4-hydroxy-3-nitrobenzyl alcohol is 1:3.5.
[0048] Embodiment 4:
[0049] The difference between the preparation method of a mixed decolorizing agent and Example 1 is that dicyandiamide formaldehyde resin polymer is used instead of modified dicyandiamide formaldehyde resin polymer.
[0050] Embodiment 5:
[0051] The difference between the preparation method of a mixed decolorizing agent and Example 1 is that modified diatomaceous earth is used instead of diatomaceous earth.
[0052] The preparation method of modified diatomite comprises the following steps:
[0053] Step 1: add ethanol to diatomaceous earth (the mass volume ratio of diatomaceous earth to ethanol is: 1 g: 10 mL), then slowly add γ-glycidyloxypropyltrimethoxysilane at 38°C, react at constant temperature for 7 hours, filter, wash with ethanol, and dry to obtain condensation-modified diatomaceous earth;
[0054] Step 2: Add distilled water, tetrahydrofuran and cobalt acetate tetrahydrate to the condensed modified diatomaceous earth, stir and mix at 0°C for 20 hours, then naturally warm to room temperature, stand for 20 hours, filter, wash with ethanol three times, and dry to obtain open-ring diatomaceous earth;
[0055] Step 3: Add thionyl chloride to the opened diatomaceous earth, then add p-carboxybenzenesulfonamide, stir and mix evenly, react at 100° C. for 5 h, wash with distilled water 3 times, and wash with methanol 3 times to obtain modified diatomaceous earth.
[0056] Wherein, the ethanol in step one is an ethanol aqueous solution with a concentration of 80wt%; in step one, the mass volume ratio of diatomite to γ-glycidyloxypropyltrimethoxysilane is: 1g:3mL. In step two, the mass volume ratio of condensation-modified diatomite to distilled water is: 1g:10mL, the mass volume ratio of condensation-modified diatomite to tetrahydrofuran is: 1g:0.15mL, and the mass ratio of condensation-modified diatomite to cobalt acetate tetrahydrate is: 1:0.005. In step three, the mass volume ratio of open-loop diatomite to dichlorothionyl is: 1g:40mL; the mass ratio of open-loop diatomite to p-carboxybenzenesulfonamide is: 1:2.5.
[0057] Embodiment 6:
[0058] The difference between the preparation method of a mixed decolorizing agent and Example 4 is that modified diatomaceous earth is used instead of diatomaceous earth.
[0059] The preparation method of modified diatomaceous earth is the same as that in Example 5.
[0060] Embodiment 7:
[0061] The difference between the preparation method of a mixed decolorizing agent and Example 1 is that the preparation method of the modified dicyandiamide formaldehyde resin polymer is different.
[0062] The difference between the preparation method of the modified dicyandiamide formaldehyde resin polymer and Example 1 is that methanol is used instead of 4-hydroxy-3-nitrobenzyl alcohol.
[0063] Embodiment 8:
[0064] The difference between a method for preparing a mixed decolorizing agent and Example 6: the preparation method of the modified diatomaceous earth is different.
[0065] The difference between the preparation method of modified diatomaceous earth and Example 6 is that 3-carboxybenzaldehyde is used instead of p-carboxybenzenesulfonamide.
[0066] Test example:
[0067] 1. Infrared spectrum test
[0068] The samples were analyzed by potassium bromide pellet method and Fourier transform infrared spectrometer.
[0069] The above test was performed on the modified dicyandiamide formaldehyde resin polymer and dicyandiamide formaldehyde resin polymer prepared in Example 1. The results are as follows: Figure 1 As shown. Figure 1 It can be seen that compared with the infrared spectrum of dicyandiamide formaldehyde resin polymer, the infrared spectrum of modified dicyandiamide formaldehyde resin polymer is at 1510 cm -1 、1339cm -1There are antisymmetric and symmetric stretching absorption peaks of nitro group at , indicating that 4-hydroxy-3-nitrobenzyl alcohol participates in the formation reaction of modified dicyandiamide formaldehyde resin polymer.
[0070] The above test was performed on the modified diatomite, the ring-opened diatomite, the condensed modified diatomite and the diatomite prepared in Example 5. The results are as follows: Figure 2 As shown. Figure 2 It can be seen that compared with the infrared spectrum of diatomite, the infrared spectrum of condensed modified diatomite is at 911cm -1 The infrared characteristic absorption peak of epoxy group exists at 911cm -1 The infrared characteristic absorption peak of the epoxy group at the position disappears, indicating that the condensation-modified diatomite undergoes a ring-opening reaction to generate open-ring diatomite; the infrared spectrum of the modified diatomite is at 1400-1600cm -1 The presence of the infrared characteristic absorption peak of the benzene ring indicates that p-carboxybenzenesulfonamide participates in the formation reaction of modified diatomite.
[0071] 2. Decolorization effect test
[0072] In the wastewater with K-type active dye concentration of 1000mg / L, add the mixed decolorant sample at a dosage of 200mg / L, and use the dilution multiple method to determine the chromaticity. The decolorization rate is calculated as follows:
[0073] F / %=[(U0-U1) / U0]×100%
[0074] Among them, F is the decolorization rate; U0 is the chromaticity of the wastewater before treatment; U1 is the chromaticity of the wastewater after treatment.
[0075] Table 1 Decolorization effect test results
[0076]
[0077] The above test was performed on the mixed decolorizing agents prepared in Examples 1 to 8, and the results are shown in Table 1. As can be seen from Table 1, compared with Example 4 and Example 5 and Example 6, the decolorization rate of Example 1 is significantly improved, indicating that the dicyandiamide formaldehyde resin polymer is modified by 4-hydroxy-3-nitrobenzyl alcohol, and the modified dicyandiamide formaldehyde resin polymer is used for the preparation of the mixed decolorizer, so that the mixed decolorizer has a good decolorization effect; compared with Example 1 and Example 6, the decolorization rate of Example 5 is also significantly increased, indicating that diatomaceous earth is modified by p-carboxybenzenesulfonamide, and the modified diatomaceous earth is used for the preparation of the mixed decolorizer, so that the mixed decolorizer also has a good decolorization effect; compared with Example 7, the decolorization rate of Example 1 is also improved, indicating that the modified dicyandiamide formaldehyde resin polymer obtained by using 4-hydroxy-3-nitrobenzyl alcohol as a modifier has a better decolorization effect than conventional modified substances; compared with Example 8, the decolorization rate of Example 6 is also improved, indicating that the modified diatomaceous earth obtained by using p-carboxybenzenesulfonamide as a modifier has a better decolorization effect than conventional modified substances.
[0078] 3.COD removal effect test
[0079] A mixed decolorant sample was added to wastewater with a COD concentration of 900 mg / L in an amount of 200 mg / L. The COD content before and after wastewater treatment was tested using the potassium dichromate method. The COD removal rate calculation formula was the same as in Test Example 2.
[0080] Table 2 COD removal effect test results
[0081]
[0082] The above test was performed on the mixed decolorizing agents prepared in Examples 1 to 8, and the results are shown in Table 2. As can be seen from Table 2, compared with Example 4 and Example 5 and Example 6, the COD removal rate of Example 1 is significantly improved, indicating that the dicyandiamide formaldehyde resin polymer is modified by 4-hydroxy-3-nitrobenzyl alcohol, and the modified dicyandiamide formaldehyde resin polymer is used for the preparation of the mixed decolorizer, so that the mixed decolorizer has a good COD removal effect; compared with Example 1 and Example 6, the COD removal rate of Example 5 is also significantly increased, indicating that diatomaceous earth is modified by p-carboxybenzenesulfonamide, and the modified diatomaceous earth is used for the preparation of the mixed decolorizer, so that the mixed decolorizer also has a good COD removal effect; compared with Example 7, the COD removal rate of Example 1 is also improved, indicating that the modified dicyandiamide formaldehyde resin polymer obtained by using 4-hydroxy-3-nitrobenzyl alcohol as a modifier has a better COD removal effect than conventional modified substances; compared with Example 8, the COD removal rate of Example 6 is also improved, indicating that the modified diatomaceous earth obtained by using p-carboxybenzenesulfonamide as a modifier has a better COD removal effect than conventional modified substances.
[0083] 4. Ammonia nitrogen removal effect test
[0084] A mixed decolorant sample was added to wastewater with an ammonia nitrogen content of 550 mg / L in an amount of 200 mg / L. The ammonia nitrogen content before and after the wastewater treatment was tested by spectrophotometry. The ammonia nitrogen removal rate calculation formula was the same as that in Test Example 2.
[0085] Table 3 Ammonia nitrogen removal effect test results
[0086]
[0087] The above test was performed on the mixed decolorizing agents prepared in Examples 1 to 8, and the results are shown in Table 3. As can be seen from Table 3, compared with Example 4 and Example 5 and Example 6, the ammonia nitrogen removal rate of Example 1 is significantly improved, indicating that the dicyandiamide formaldehyde resin polymer is modified by 4-hydroxy-3-nitrobenzyl alcohol, and the modified dicyandiamide formaldehyde resin polymer is used for the preparation of the mixed decolorizer, so that the mixed decolorizer has a good ammonia nitrogen removal effect; compared with Example 1 and Example 6, the ammonia nitrogen removal rate of Example 5 is also significantly increased, indicating that diatomaceous earth is modified by p-carboxybenzenesulfonamide, and the modified diatomaceous earth is used for the preparation of the mixed decolorizer, so that the mixed decolorizer also has a good ammonia nitrogen removal effect; compared with Example 7, the ammonia nitrogen removal rate of Example 1 is also improved, indicating that the modified dicyandiamide formaldehyde resin polymer obtained by using 4-hydroxy-3-nitrobenzyl alcohol as a modifier has a better ammonia nitrogen removal effect than conventional modified substances; compared with Example 8, the ammonia nitrogen removal rate of Example 6 is also improved, indicating that the modified diatomaceous earth obtained by using p-carboxybenzenesulfonamide as a modifier has a better ammonia nitrogen removal effect than conventional modified substances.
[0088] The conventional techniques in the above embodiments are prior arts known to those skilled in the art, and thus will not be described in detail here.
[0089] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A modified dicyandiamide formaldehyde resin polymer, characterized in that: The modified dicyandiamide formaldehyde resin polymer comprises a dicyandiamide formaldehyde resin polymer and a surface modification group thereof; the surface modification group is 4-hydroxy-3-nitrobenzyl alcohol, and etherification reaction occurs between 4-hydroxy-3-nitrobenzyl alcohol and the dicyandiamide formaldehyde resin polymer.
2. A mixed decolorizing agent comprising the modified dicyandiamide formaldehyde resin polymer according to claim 1.
3. A mixed decolorizing agent according to claim 2, characterized in that: The mixed decolorizing agent also contains polydimethyldiallylammonium chloride, polyferric sulfate, polyaluminum sulfate, diatomaceous earth, activated carbon and aluminum sulfate.
4. A mixed decolorizing agent according to claim 3, characterized in that: In the mixed decolorizing agent, by weight, the amount of modified dicyandiamide formaldehyde resin polymer is 20 to 50 parts, the amount of polydimethyldiallylammonium chloride is 1 to 5 parts, the amount of polyferric sulfate is 1 to 3 parts, the amount of polyaluminum sulfate is 1 to 3 parts, the amount of diatomaceous earth is 1 to 3 parts, the amount of activated carbon is 2 to 8 parts, and the amount of aluminum sulfate is 2 to 6 parts.
5. The method for preparing the modified dicyandiamide formaldehyde resin polymer according to claim 1, characterized in that: The molar ratio of the dicyandiamide formaldehyde resin polymer to 4-hydroxy-3-nitrobenzyl alcohol is 1:3-4.
6. Use of the modified dicyandiamide formaldehyde resin polymer according to claim 1 in the preparation of a decolorizing agent.
7. Use of the modified dicyandiamide formaldehyde resin polymer according to claim 1 in the treatment of wastewater in the liquid crystal display manufacturing industry.