A rubber-plastic composite sealing plate and its preparation method and application
By injecting and vulcanizing rubber in the rubber groove of the liquid flow battery sealing plate frame, the integrated rubber-plastic composite sealing plate is solved, and the sealing performance and acid and alkali resistance are improved Performance, simplifies the processing process and reduces costs.
Patent Information
- Application Number
- CN202311799361.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-12-25
AI Technical Summary
The bond between the existing flow battery sealing plate frame and the rubber sealing strip is not firm, resulting in poor sealing performance, and the installation process is time-consuming and labor-intensive and has low accuracy, which can easily lead to increased battery internal resistance and reduced sealing performance.
By controlling the injection temperature, the unvulcanized rubber is directly injected into the rubber groove of the battery sealing plate frame, and cured and cross-linked to form an integrated rubber-plastic composite sealing plate, avoiding glue Deformation and structural damage caused by bonding and high temperatures.
It realizes the efficient sealing performance of rubber-plastic composite sealing plates and long-term acid and alkali resistance performance, simplifies the processing process, reduces production costs, avoids the accuracy of bonding and installation of sealing strips, and prevents fluorine and sulfur elements. introduction.
Smart Images

Figure CN117863447B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sealing materials, and in particular to a rubber-plastic composite sealing plate and a preparation method and application thereof. Background Art
[0002] The battery sealing plate is a sealing material used in the field of battery sealing. It can avoid problems such as leakage of electrolyte in the battery and has a key impact on the performance and service life of the battery. For example, when the sealing performance of the battery sealing plate to the liquid flow battery is insufficient, it will cause the electrolyte to leak, and the battery performance and life will be seriously affected. In order to ensure the sealing effect of the liquid flow battery, it is necessary to design a serpentine flow channel and a sealing strip that cooperate with each other on the plate frame of the liquid flow battery electrode sealing plate. The material of the sealing strip is generally rubber, which is mainly divided into two types: line sealing and surface sealing. At present, the sealing plate frame of the liquid flow battery mainly adopts general plastics such as polyethylene (PE) or polypropylene (PP), but the surface groups of these materials are inert and not easy to bond with the rubber sealing strip, resulting in poor sealing performance of the sealing plate to the overall liquid flow battery. Therefore, how to accurately fix the sealing strip on both sides of the sealing plate frame, and at the same time ensure that the sealing strip does not fall off and is easy to position when the battery stack (battery pack) is assembled, is one of the key links to determine the sealing performance of the liquid flow battery and its battery stack.
[0003] In the prior art, glue is generally used to bond the sealing strip to the sealing plate frame, or the sealing strip is installed in a rubber groove. However, the glue is corroded by the electrolyte and enters the electrolyte to form impurities. In severe cases, elements such as fluorine and sulfur will be introduced, resulting in increased internal resistance of the battery and reduced sealing performance. It is also difficult to ensure the sealing performance by simply installing the sealing strip in the rubber groove. In addition, the process of gluing or installing it in the rubber groove is time-consuming and labor-intensive, and the accuracy is also low.
[0004] Therefore, developing sealing plates composed of rubber sealing strips and plastic sealing plate frames to solve the installation and positioning problems of sealing strips is a development trend in flow battery sealing materials and structural design, and is of great significance to the development of flow battery technology. Summary of the invention
[0005] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, the purpose of the present invention is to provide a method for preparing a rubber-plastic composite sealing plate, by controlling the injection temperature, directly injecting unvulcanized rubber into the rubber groove of the plate frame, and then controlling the vulcanization temperature so that the rubber is cured and cross-linked in the rubber groove of the sealing plate frame.
[0006] A second aspect of the present invention is to provide a rubber-plastic composite sealing plate.
[0007] The third aspect of the present invention is to provide an application of a rubber-plastic composite sealing plate.
[0008] A fourth aspect of the present invention is to provide a liquid flow battery.
[0009] In order to achieve the above object, the technical solution adopted by the present invention is:
[0010] The first aspect of the present invention is to provide a method for preparing a rubber-plastic composite sealing plate, comprising the following steps:
[0011] S1. The plastic is injection molded to obtain a battery sealing frame containing a rubber groove, and cooled;
[0012] S2. The unvulcanized rubber containing a cross-linking agent is injection molded into the rubber groove of the battery sealing plate frame and vulcanized to obtain a rubber-plastic composite sealing plate;
[0013] The value of the heat deformation temperature of the plastic minus the injection temperature of the rubber is ≥35°C;
[0014] The value obtained by subtracting the vulcanization temperature of the rubber from the heat deformation temperature of the plastic is ≥30°C.
[0015] The present invention injects unvulcanized rubber into the rubber groove of the battery sealing plate frame, and then performs vulcanization, so that the rubber is directly cured and cross-linked in the rubber groove of the battery sealing plate frame to form a sealing strip, thereby obtaining an integrally formed rubber-plastic composite sealing plate. In this process, the injection temperature and vulcanization temperature of the rubber need to be strictly controlled. When the injection temperature or the vulcanization temperature is too high, the deformation of the battery sealing plate frame will be too large, and obvious warping deformation will occur, and it cannot be used as a sealing plate. At the same time, during the injection molding process, due to the high temperature, the rubber groove of the battery sealing plate frame will be broken, and the rubber will penetrate into the plate from the plate frame, destroying other functional structures and affecting the long-term acid and alkali medium resistance of the rubber-plastic composite sealing plate.
[0016] The rubber-plastic composite sealing plate obtained by the present invention is integrally formed by injection molding, and has good composite properties. The rubber and the battery sealing plate frame do not need to be bonded by gluing, thereby improving the sealing performance of the rubber-plastic composite sealing plate. At the same time, injection molding the rubber into the rubber groove can also reduce the trimming process, reduce the deformation of the battery sealing plate frame during the processing process, and avoid the problem that the rubber sealing strip is difficult to position during bonding or installation, and the sealing strip is easily misplaced when the battery stack is stacked.
[0017] The heat deformation temperature of plastics is generally within a range. At this time, the lower limit of the heat deformation temperature range of plastics is used to compare with the injection temperature and vulcanization temperature of rubber.
[0018] In some embodiments of the present invention, the value of the heat deformation temperature of the plastic minus the injection temperature of the rubber is 40-140°C.
[0019] In some embodiments of the present invention, the value of the heat deformation temperature of the plastic minus the vulcanization temperature of the rubber is ≥35°C.
[0020] In some embodiments of the present invention, the value of the heat deformation temperature of the plastic minus the vulcanization temperature of the rubber is 35-50°C.
[0021] In some embodiments of the present invention, the injection temperature of the rubber in step S2 is 30-140°C.
[0022] In some embodiments of the present invention, the injection temperature of the rubber in step S2 is 90-110°C.
[0023] In some embodiments of the present invention, the vulcanization temperature of the rubber in step S2 is 90-195°C.
[0024] In some embodiments of the present invention, the vulcanization temperature of the rubber in step S2 is 115-180°C.
[0025] When the material of the battery sealing plate frame, that is, the plastic in step S1 is engineering plastic, such as polysulfone, polyamide, polyphenylene ether, etc., the heat deformation temperature of the plastic is relatively high, and the injection temperature and vulcanization temperature of the rubber are controlled below 200°C; when the material of the battery sealing plate frame, that is, the plastic in step S1 is general plastic, such as polyethylene, polypropylene, etc., the heat deformation temperature of the plastic is relatively low, and the injection temperature and vulcanization temperature of the rubber need to be controlled below 150°C.
[0026] In the preparation method of the present invention, the vulcanization temperature of the rubber and its injection temperature are coordinated with each other, and the vulcanization temperature of the rubber is generally not lower than the injection temperature of the rubber.
[0027] If the rubber itself requires a higher vulcanization temperature, the vulcanization temperature of the rubber can be lowered by adding a low-temperature cross-linking agent.
[0028] Low-temperature crosslinking agent refers to a type of crosslinking agent with a typical initiation temperature below 150°C that can (or can, with the synergistic effect of an auxiliary agent) initiate a crosslinking and curing reaction of a polymer material.
[0029] In some embodiments of the present invention, the low-temperature crosslinking agent is one or more combinations of lauroyl peroxide (LPO), tert-butyl perbenzoate (TBPB), di(2,4-dichlorobenzoyl) peroxide (DCBP), and dibenzoyl peroxide (BPO).
[0030] In some embodiments of the present invention, the injection pressure of the rubber in step S2 is 5-40 MPa.
[0031] In some embodiments of the present invention, the injection pressure of the rubber in step S2 is 8-20 MPa.
[0032] By controlling the injection pressure, it is possible to further ensure that the rubber is successfully injected into the rubber groove of the battery sealing plate frame during injection, while ensuring the filling of the rubber, further preventing the rubber from penetrating into the plate and destroying other functional structures, resulting in a decrease in sealing performance and long-term acid and alkali medium resistance.
[0033] In some embodiments of the present invention, the rubber injection process in step S2 is performed under pressure maintenance for 5 to 10 minutes; the pressure of the pressure maintenance is the injection pressure.
[0034] In some embodiments of the present invention, the vulcanization process in step S2 is performed under pressure for 3 to 30 minutes; the pressure of the pressure maintenance is ≤20 MPa.
[0035] The vulcanization process after injection is performed by maintaining pressure for a certain period of time to ensure that the rubber sealing strip is fully and evenly cross-linked, so that the size, structure and position of each part are within the design tolerance range, and there are no defects such as stains and damage on the surface.
[0036] In some embodiments of the present invention, the holding pressure of the vulcanization process is 8-20 MPa.
[0037] In some specific embodiments of the present invention, the holding pressure of the vulcanization process is 6-15 MPa.
[0038] In some embodiments of the present invention, the vulcanization process in step S2 is performed under pressure for 3 to 10 minutes.
[0039] In some specific embodiments of the present invention, the vulcanization process in step S2 is performed under pressure for 5 to 7 minutes.
[0040] In some embodiments of the present invention, the compression rate of the rubber after injection in step S2 is 10-30%.
[0041] In some embodiments of the present invention, the compression rate of the rubber after injection in step S2 is 15-25%.
[0042] In some specific embodiments of the present invention, the compression rate of the rubber after injection in step S2 is 20%.
[0043] In some embodiments of the present invention, the filling rate of the rubber in the rubber groove in step S2 is above 80%.
[0044] In some embodiments of the present invention, the filling rate of the rubber in the rubber groove in step S2 is 82-95%.
[0045] In some specific embodiments of the present invention, the filling rate of the rubber in the rubber groove in step S2 is 90-95%.
[0046] In some embodiments of the present invention, the cooling in step S1 is performed at room temperature to eliminate the residual internal stress of the battery sealing plate frame.
[0047] In some embodiments of the present invention, in step S1, annealing is performed first and then cooling is performed.
[0048] In some embodiments of the present invention, the annealing treatment is performed at a temperature of 160-190°C.
[0049] In some embodiments of the present invention, the width of the flash generated after the rubber is vulcanized is ≤0.5 mm.
[0050] By controlling the burr width, the influence of the burr on the battery life under long-term use can be avoided.
[0051] In some embodiments of the present invention, the width of the flash generated by the rubber after vulcanization molding is ≤0.3 mm.
[0052] In some embodiments of the present invention, the plastic includes polyethylene, polypropylene, polysulfone, polyamide, and polyphenylene ether.
[0053] In some embodiments of the present invention, the rubber is an acid and alkali resistant rubber, specifically including fluorosilicone, EPDM rubber, fluororubber, hydrogenated nitrile rubber, perfluoroether rubber, polyisobutylene rubber, and tetrafluoroethylene rubber.
[0054] In some embodiments of the present invention, the fluororubber is peroxide fluororubber.
[0055] In some embodiments of the present invention, the cross-linking agent is at least one of dilauroyl peroxide, dicumyl peroxide (DCP), and di-tert-butylcumyl peroxide (BIPB).
[0056] In some embodiments of the present invention, the injection molding temperature of the plastic in step S1 is 200-350°C.
[0057] In some embodiments of the present invention, the injection molding temperature of the plastic in step S1 is 200°C, 210°C, 220°C, or 300°C.
[0058] In some embodiments of the present invention, the battery sealing plate frame obtained in step S1 contains a sealing strip, positioning holes, and a flow channel.
[0059] During the preparation process, the rubber is injected into the rubber groove, and after vulcanization, it is cured and cross-linked to form a sealing strip.
[0060] In some embodiments of the present invention, the cross-section of the sealing strip is at least one of a rectangular shape, a circular shape, a "D" shape, and a "convex" shape.
[0061] In some embodiments of the present invention, the flow channel includes an electrolyzed water inlet, a hydrogen outlet, and an electrolyzed water and oxygen outlet, and a sealing strip forms a sealing ring around the flow channel, and the sealing ring is a wire seal.
[0062] The sealing ring comprises a rubber groove and a rubber sealing strip which is solidified and formed in the rubber groove.
[0063] The second aspect of the present invention provides a rubber-plastic composite sealing plate prepared by the preparation method described in the first aspect of the present invention.
[0064] The third aspect of the present invention provides an application of the rubber-plastic composite sealing plate described in the second aspect of the present invention in the field of battery sealing.
[0065] A fourth aspect of the present invention provides a liquid flow battery, comprising the rubber-plastic composite sealing plate according to the second aspect of the present invention.
[0066] In some embodiments of the present invention, the liquid flow battery further comprises an electrolyte.
[0067] In some embodiments of the present invention, the electrolyte is a concentrated ferrous hydrochloride electrolyte or a concentrated vanadium sulfate electrolyte.
[0068] Compared with the prior art, the present invention has at least the following beneficial technical effects:
[0069] (1) The present invention controls the injection molding temperature and the vulcanization temperature during the preparation process, thereby successfully injecting the rubber into the rubber groove of the battery sealing plate frame, ensuring that the battery sealing plate frame does not undergo significant deformation, and preventing the rubber from breaking through the rubber groove and damaging other functional structures, thereby realizing an integrated structure of the rubber-plastic composite sealing plate, improving the sealing performance and long-term acid and alkali resistance of the rubber-plastic composite sealing plate, and the preparation method is simple, does not require any machining or assembly operations, and has a low production cost.
[0070] (2) The rubber-plastic composite sealing plate obtained by the present invention has an integrally formed composite structure, and the battery sealing plate frame and the rubber sealing strip are well composited, thereby improving the sealing performance and long-term acid and alkali medium resistance of the rubber-plastic composite sealing plate, avoiding the problem of difficulty in positioning the rubber sealing strip during bonding or installation, and the problem of easy misalignment of the sealing strip during battery stacking.
[0071] (2) The rubber-plastic composite sealing plate obtained by the present invention has good sealing performance and long-term acid and alkali medium resistance, does not require glue bonding, and will not introduce fluorine and sulfur elements to increase the internal resistance of the battery. It is suitable as a battery sealing material, especially suitable for the field of liquid flow battery sealing. BRIEF DESCRIPTION OF THE DRAWINGS
[0072] Figure 1 This is a schematic diagram of the combination of the rubber-plastic composite sealing plate frame and the sealing strip according to Example 1 of the present invention.
[0073] Figure 2 This is an exploded view of the plastic plate frame and the sealing strip according to Example 1 of the present invention.
[0074] Figure 3 This is a schematic diagram of a plastic frame according to Example 1 of the present invention.
[0075] Figure 4 This is a schematic diagram of the sealing strip according to Example 1 of the present invention.
[0076] Figure 5 This is a cross-sectional view of the upper electrode plate and the lower electrode plate of the tooling in the initial sealing test of an embodiment of the present invention; from left to right are the upper electrode plate and the lower electrode plate.
[0077] Figure 6 It is a schematic diagram of the assembly of the tooling in the initial sealing test of an embodiment of the present invention.
[0078] Figure 7 It is a schematic diagram of the structure after the tooling is assembled in the initial sealing test of an embodiment of the present invention.
[0079] The numbers in the accompanying drawings are explained as follows:
[0080] Figure 1 Middle: 1-plastic plate frame; 2-sealing strip; 3-flow channel; 4-positioning hole;
[0081] Figure 3 Middle: 5-Seal groove. DETAILED DESCRIPTION
[0082] The present invention is further described in detail below by specific examples. Unless otherwise specified, the raw materials, reagents or devices used in the examples and comparative examples can be obtained from conventional commercial sources or can be obtained by prior art methods. Unless otherwise specified, the experiments or test methods are conventional methods in the art.
[0083] The test methods of the following embodiments and comparative examples of the present invention are described as follows:
[0084] The sealing performance and long-term acid and alkali resistance are tested through the following steps:
[0085] 1. Initial sealing test: After assembling 5 to 6 rubber-plastic composite sealing plates with the tooling, test the water tightness at room temperature, high temperature (80°C), and low temperature (2°C) in sequence; when testing water tightness, put the tooling with the rubber-plastic composite sealing plates into the corresponding temperature oven, balance for 2 hours, and then apply 0.5MPa water pressure. If there is no liquid seepage, proceed to step 2;
[0086] The main body of the test fixture used is composed of two metal plates and four sets of screws and nuts of different lengths. The metal plates are divided into A plate and B plate. Both A plate and B plate are alloy plates. A tapered pipe threaded hole is opened in the center of the plate, and standard O-ring grooves are opened on the inner wall surface around it. Figure 5 As shown;
[0087] The assembly of the tooling is mainly divided into three parts: the lower plate, the middle rubber-plastic composite sealing plate sample and the upper plate. The rubber-plastic composite sealing plates are stacked in 5 to 6 groups; Figure 6 As shown;
[0088] The lower electrode plate, the middle rubber-plastic composite sealing plate sample and the upper electrode plate are stacked vertically. The structure after stacking is as follows Figure 7 As shown; one side is connected to the pressure inlet side, and the other side is connected to the pressure outlet side. The pressure inlet side can be connected to the oil circuit or compressed air for pressurization, and the pressure outlet side can be connected to a pressure gauge or a throttle valve; finally, it is assembled and fixed by a combination of screws and nuts.
[0089] 2. Long-term acid and alkali resistance test: Pour the corresponding acid and alkali media into the tooling equipped with the rubber-plastic composite sealing plate, put it in an oven, and age it for 500 hours;
[0090] The first acid medium is concentrated vanadium sulfate electrolyte, and the operating temperature is 40°C, so the oven temperature is set to 50°C to accelerate aging;
[0091] The second acid medium is concentrated ferrous hydrochloride electrolyte, and the operating temperature is 60-80°C, so the oven temperature is set to 80°C to accelerate aging;
[0092] The alkaline medium is a sodium hydroxide solution with a pH of 14 and a use temperature of 60-80°C, so the oven temperature is set at 80°C to accelerate aging;
[0093] During specific testing, select the appropriate medium based on the application scenario;
[0094] If there is no obvious leakage, proceed to step 3;
[0095] 3. Sealing test: After pouring out the acid and alkali media, perform a sealing test. The test method is the same as step 1. If there is no liquid seepage, proceed to step 4.
[0096] 4. Long-term acid and alkali resistance test: Pour the corresponding acid and alkali medium, put it in an 80℃ oven, and age it for 500h; the acid and alkali medium are the same as step 2, and the set temperature is changed to 80℃; if there is no obvious leakage, proceed to step 5;
[0097] 5. Sealing test: Pour out the acid and alkali media, and then conduct a sealing test. The test method is the same as step 1. Observe whether there is liquid seepage;
[0098] After the above-mentioned simulated loading and sealing and long-term acid and alkali medium resistance cycle tests, the aging time is 1000h in total. If there is no obvious leakage, it is judged that the sealing performance of the rubber-plastic composite sealing plate meets the standards.
[0099] The compression rate of rubber can be calculated as follows: 1-compressed height / uncompressed height.
[0100] The filling rate of rubber can be obtained by the following calculation method: product cross-sectional area / groove cross-sectional area.
[0101] Example 1
[0102] This embodiment provides a method for preparing a rubber-plastic composite sealing plate, comprising the following steps:
[0103] Put polypropylene pellets into the barrel of an injection molding machine for heating, perform injection molding at 210°C, and perform injection molding at a pressure of 65MPa. After injection molding, place the material at room temperature for 8 hours for cooling. After the internal stress is completely released, a battery sealing plate frame is obtained. Unvulcanized EPDM rubber is injected into the rubber groove of the battery sealing plate frame at 110°C. The injection pressure of the rubber is 8MPa. The pressure holding time of the injection process is 7min. After the rubber is injected, vulcanization is performed at 115°C, and a pressure of 6MPa is maintained for 5min, so that the rubber is cured and cross-linked in the rubber groove to form a sealing strip, thereby obtaining a rubber-plastic composite sealing plate.
[0104] The compression rate of the vulcanized rubber is 25% and the filling rate is 93%. The flash produced by the rubber sealing strip molding is within 0.2 mm and is accommodated in the groove of the double-layer structure.
[0105] Among them, a low-temperature cross-linking agent, dilauroyl peroxide, is added to the unvulcanized rubber; the heat deformation temperature of the polypropylene pellets is around 150°C.
[0106] The rubber-plastic composite sealing plate obtained in this embodiment has a battery sealing plate frame, a rubber groove on the battery sealing plate frame and a sealing strip in the rubber groove; the sealing strip is an EPDM rubber initiated by a dilauroyl peroxide (LPO) vulcanization system, and the battery sealing plate frame also contains flow channels and positioning holes. The positioning holes are arranged along the outer edge of the battery sealing plate frame. The cross-section of the rubber sealing strip is rectangular, which is used to seal the ion exchange membrane and the electrode plate frame to prevent leakage of the electrolyte inside the cavity, which affects the current density of the battery and the service life of the battery stack.
[0107] Example 2
[0108] This embodiment provides a method for preparing a rubber-plastic composite sealing plate, comprising the following steps:
[0109] Put polyphenylene ether (NORYL GFN30F) pellets into the barrel of an injection molding machine for heating, perform injection molding at 280-320°C, the injection molding pressure is 87MPa, the injection mold temperature is 120-140°C, annealing treatment is performed at 160-190°C for 4h after injection molding, and then placed at room temperature for 8h for cooling, and the battery sealing plate frame is obtained after the internal stress is completely released, and unvulcanized peroxide fluororubber (PFR5920M) is injected into the rubber groove of the battery sealing plate frame at 90°C, the injection pressure of the rubber is 20MPa, and the pressure holding time of the injection process is 7min. After the rubber is injected, it is vulcanized at 180°C, and the pressure of 15MPa is maintained for 7min, so that the rubber is cured and cross-linked in the rubber groove to form a sealing strip, and a rubber-plastic composite sealing plate is obtained;
[0110] Among them, the cross-linking agent di-tert-butyl peroxide isopropylbenzene (BIPB) is added to the unvulcanized rubber; the thermal deformation of the polyphenylene ether pellets is above 230°C; the compression rate of the rubber in the rubber groove after injection molding is 20%, and the filling rate is 95%; the flash generated by the molding of the rubber sealing strip is within 0.3mm.
[0111] The rubber-plastic composite sealing plate obtained in this embodiment has a battery sealing plate frame, a rubber groove on the battery sealing plate frame and a sealing strip in the rubber groove; the sealing strip is a peroxide fluororubber initiated by a di-tert-butyl peroxide isopropylbenzene vulcanization system, and the battery sealing plate frame also contains a flow channel and a positioning hole, the positioning holes are arranged along the outer edge of the battery sealing plate frame, the battery sealing plate frame contains a flow channel and a sealing ring formed around it, the sealing ring is a line seal, and the line seal refers to the rubber sealing strip in the rubber groove; the cross-section of the rubber sealing strip is a "convex" shape, enclosing the electrolyte flow channel in the battery sealing plate frame, and is used to seal the ion exchange membrane and the electrode plate frame to prevent the electrolyte inside the cavity from leaking, affecting the current density of the battery and the service life of the battery stack; there is no reinforcing rib structure on the plate frame surface.
[0112] Comparative Example 1
[0113] This comparative example provides a method for preparing a rubber-plastic composite sealing plate, and the steps are the same as those of Example 1, except that the injection temperature of the rubber is 120°C.
[0114] The structure of the rubber-plastic composite sealing plate is the same as that of Example 1.
[0115] Comparative Example 2
[0116] This comparative example provides a method for preparing a rubber-plastic composite sealing plate, and the steps are the same as those of Example 1, except that the injection temperature of the rubber is 130°C.
[0117] The structure of the rubber-plastic composite sealing plate is the same as that of Example 1.
[0118] Results
[0119] The sealing performance and long-term acid and alkali resistance of the rubber-plastic composite sealing plate obtained in the above embodiment were tested, and the results are as follows:
[0120] For Example 1, according to the corresponding application scenario, 50°C concentrated vanadium sulfate electrolyte was selected for sealing performance-long-term acid and alkali resistance cycle test, and 5 rubber-plastic composite sealing plates were randomly selected from the same batch and assembled into a test pile. After cyclic aging for a total of 1000 hours according to the test method recorded in steps 1 to 5 above, it can still seal 1.4MPa water pressure, the sealing performance is qualified, and the long-term acid and alkali resistance performance is good.
[0121] For Example 2, according to the corresponding application scenario, 80°C concentrated ferrous hydrochloride electrolyte was selected for sealing performance test, and 5 rubber-plastic composite sealing plates were randomly selected from the same batch and assembled into a test pile. After cyclic aging for a total of 2000 hours according to the test method recorded in steps 1 to 5 above, it can still seal 1MPa water pressure, the sealing performance is qualified, and the long-term acid and alkali medium resistance performance is good.
[0122] When the injection temperature of the rubber in Comparative Example 1 was too high, the deformation of the battery sealing plate frame was greater than 5 mm, and obvious warping deformation occurred; when the injection temperature of the rubber in Comparative Example 2 was further increased, the battery sealing plate frame was broken, the injection pressure dropped suddenly, and the rubber infiltrated and destroyed other functional structures. Therefore, Comparative Examples 1 and 2 could not successfully obtain a rubber-plastic composite sealing plate with good sealing performance and long-term acid and alkali medium resistance.
[0123] In summary, the preparation method of the present invention can successfully inject the rubber into the rubber groove of the battery sealing plate frame, and ensure that the battery sealing plate frame does not undergo obvious deformation, while preventing the rubber from breaking through the rubber groove and damaging other functional structures, thereby realizing the integrated structure of the rubber-plastic composite sealing plate, improving the sealing performance and long-term acid and alkali medium resistance of the rubber-plastic composite sealing plate, and the preparation method is simple, does not require any machining or assembly operations, and has low production costs. The obtained rubber-plastic composite sealing plate is particularly suitable for the field of liquid flow battery sealing.
[0124] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a rubber-plastic composite sealing plate, It is characterized in that The steps include: S1. The plastic is injection molded to obtain a battery sealing frame containing a rubber groove, and cooled; S2. The unvulcanized rubber containing a cross-linking agent is injected into the rubber groove of the battery sealing plate frame and vulcanized to obtain a rubber-plastic composite sealing plate; The value of the heat deformation temperature of the plastic minus the injection temperature of the rubber is ≥35°C; The value of the heat deformation temperature of the plastic minus the vulcanization temperature of the rubber is ≥30°C; The injection pressure of the rubber in step S2 is 5-40 MPa; The vulcanization process in step S2 is carried out under pressure for 3 to 30 minutes; the pressure of the pressure maintenance is 6 to 20 MPa.
2. The preparation method according to claim 1, It is characterized in that The injection temperature of the rubber in step S2 is 30-140°C; And / or, the vulcanization temperature of the rubber in step S2 is 90-195°C.
3. The preparation method according to claim 1, It is characterized in that In the step S1, annealing treatment is first performed and then cooling is performed.
4. The preparation method according to claim 1, It is characterized in that The width of the flash produced after the rubber is vulcanized is ≤0.5mm.
5. The preparation method according to claim 1, It is characterized in that The plastics include polyethylene, polypropylene, polysulfone, polyamide, and polyphenylene ether; And / or, the rubber includes fluorosilicone, EPDM rubber, fluorine rubber, hydrogenated nitrile rubber, perfluoroether rubber, polyisobutylene rubber, tetrafluoroethylene rubber.
6. The preparation method according to claim 1, It is characterized in that The battery sealing plate frame obtained in step S1 contains a sealing strip, positioning holes, and a flow channel.
7. A rubber-plastic composite sealing plate prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the rubber-plastic composite sealing plate according to claim 7 in the field of battery sealing.
9. A flow battery, It is characterized in that Including the rubber-plastic composite sealing plate as described in claim 7.