A method for preparing a carbon ceramic brake disc and its product

Through composite catalytic process and silicon permeation treatment, the problems of complex and high cost of traditional carbon ceramic brake disc preparation process are solved, the graphitization degree and performance of the brake disc are improved, the hardness and crack resistance are achieved, and the manufacturing is reduced. cost.

CN117865710BActive Publication Date: 2024-12-06深圳市佰斯倍新材料科技有限公司

Patent Information

Application Number
CN202311788771.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-25
Publication Date
2024-12-06
Estimated Expiration
2043-12-25

AI Technical Summary

Technical Problem

The preparation process of traditional carbon ceramic brake discs is complex, costly and low stability, making it difficult to meet the needs of modern transportation tools to improve brake disc strength and toughness.

Method used

By using composite catalytic technology, the carbonization and low-temperature graphitization are carried out by immersing the carbon fiber preform into the phenolic resin alcohol solution by adding boron compounds. Combined with silicon permeation treatment, high-temperature silicon permeation is used to use a mixed powder of silicon powder, iron powder and nickel powder for high-temperature silicon permeation. , reduce high temperature treatment and chemical vapor deposition steps.

Benefits of technology

It reduces the difficulty of the process, improves the graphitization degree and overall performance of the carbon ceramic brake disc, reduces manufacturing costs, enhances the hardness and crack resistance of the brake disc, and improves the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004625833550000051
    Figure BDA0004625833550000051
  • Figure BDA0004625833550000111
    Figure BDA0004625833550000111
  • Figure FDA0005114656240000021
    Figure FDA0005114656240000021
Patent Text Reader

Abstract

The present invention provides a method for preparing a carbon-ceramic brake disc. By optimizing the process flow and parameters, a mixed powder of silicon powder, iron powder and nickel powder is added in the siliconizing treatment stage for siliconizing treatment. At high temperature, iron and nickel have a catalytic graphitization effect on the non-graphitized resin carbon, further improving the graphitization degree of the carbon-ceramic brake disc. At the same time, after the resin carbon with higher hardness is converted into graphite, in the process of cooling after siliconizing, the graphite also has the effect of hindering the expansion of cracks. The prepared sample has fewer cracks and higher strength, which can further improve the overall performance of the carbon-ceramic brake disc. The entire preparation process does not require chemical vapor deposition and high-temperature treatment, which can greatly reduce the process cost and improve the stability of product quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of brake disc manufacturing, and in particular to a carbon ceramic brake disc preparation method and a product thereof. Background Art

[0002] The brake materials of modern transportation vehicles such as airplanes, cars and high-speed trains have experienced a development from cast iron, synthetic materials, powder metallurgy materials to carbon-carbon composite materials and carbon-ceramic composite materials. Whether it is carbon-carbon or carbon-ceramic brake discs, their performance is actually stronger than cast iron brake discs. With the rapid development of the transportation industry, the requirements for vehicle braking performance have also increased. In addition, the area of ​​friction materials is getting smaller and smaller, and the energy per unit area of ​​friction materials is getting higher and higher, which also puts higher requirements on the strength and toughness of brake discs.

[0003] At present, the preparation process of carbon ceramic brake disc is needle puncture-carbonization-high temperature treatment-chemical vapor deposition-high temperature treatment-processing-siliconization-processing, wherein the first step of high temperature treatment is to further increase the graphitization degree of carbon fiber and remove the sizing agent on the surface of carbon fiber, and the second step of high temperature treatment is to increase the graphitization degree of chemical vapor deposition carbon to increase the friction performance of the final product. When the brake disc is in friction, the graphite on the surface has a lubricating effect, which helps to stabilize the friction coefficient, and the graphite can fill the surface holes during friction, which is conducive to forming a complete friction film and making the friction coefficient more stable. However, in the traditional process, the entire brake disc needs to be subjected to chemical vapor deposition and then graphitization treatment, which has high process cost, complex process and low stability. In this regard, a method for preparing carbon ceramic brake disc is proposed to optimize the process flow of carbon ceramic brake disc, reduce the process difficulty and have a good effect on improving the performance of the brake disc. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a carbon-ceramic brake disc and a product thereof. The difficulty of the preparation process of the carbon-ceramic brake disc is greatly reduced, and steps with high process requirements such as high-temperature treatment and chemical vapor deposition are reduced. The use of composite catalysis greatly improves the performance of the carbon-ceramic brake disc.

[0005] To achieve this object, the present invention provides a method for preparing a carbon-ceramic brake disc, and the steps for preparing the carbon-ceramic brake disc are as follows:

[0006] Step 1: preparing a carbon fiber preform of a predetermined thickness;

[0007] Step 2: impregnating the carbon fiber preform into a phenolic resin alcohol solution of a predetermined concentration, wherein the phenolic resin alcohol solution also contains a boron compound of a predetermined concentration, and forming an impregnated body after drying;

[0008] Step 3: Carbonizing the impregnated body to form a carbonized body at a carbonization temperature of 800-1100° C. for 4-6 hours;

[0009] Step 4: subjecting the carbonized body to low-temperature graphitization treatment to form a graphitized body;

[0010] Step 5: Processing the graphitized body to form a brake disc blank;

[0011] Step 6: placing the brake disc blank into a boron nitride crucible and performing siliconization treatment in a high-temperature furnace to form a silicided body, wherein the boron nitride crucible is pre-placed with filling powder, which is a mixture of silicon powder, iron powder and nickel powder;

[0012] Step 7: Processing the silicide to obtain the carbon-ceramic brake disc.

[0013] Preferably, the filler powder contains 65-90wt% silicon powder, 0.1-25wt% iron powder and 0.1-25wt% nickel powder.

[0014] Preferably, the added amount of the filling powder is 1.1 times the mass of the brake disc blank.

[0015] Preferably, the carbon fiber preform is formed by repeatedly overlapping carbon fiber unidirectional cloth and carbon fiber mesh, and each layer of unidirectional cloth and each layer of carbon fiber mesh are needle-punched after being overlapped.

[0016] Preferably, the upper and lower adjacent carbon fiber unidirectional fabrics of at least one layer of carbon fiber web are stacked at an angle of 90° in the direction of the carbon fibers.

[0017] Preferably, the acupuncture density of the acupuncture treatment is 50-200 needles / cm 2 .

[0018] Preferably, the concentration of the phenolic resin alcohol solution in step 2 is 40wt%.

[0019] Preferably, the concentration of the boron compound in step 2 is 2-5 wt %. The boron compound may be boric acid, boron oxide, boron nitride, etc.

[0020] Preferably, step 2 and step 3 are performed at least once to make the density of the carbonized body reach 1.25-1.45 g / cm 3 .

[0021] Preferably, the temperature of the low-temperature graphitization treatment in step 4 is 1400-1800° C., and the temperature is kept for 2 hours.

[0022] Preferably, the temperature of the siliconizing treatment in step 6 is 1600-1700° C., the holding time is 2-4 hours, and the pressure in the chamber of the high-temperature furnace is less than 1000 Pa.

[0023] The present invention also provides a carbon-ceramic brake disc, which contains 45-55% carbon, 40-50% silicon carbide, 8-15% silicon, 0.1-10% iron, 0.1-10% nickel and 0.5-3% boron.

[0024] Preferably, the silicon content is M Si , the total content of iron and nickel is M m , M Si and M m With the following relationship:

[0025] Preferably, the graphitization degree of the carbon-ceramic brake disc is 60-95%.

[0026] Beneficial effects: The preparation method of the carbon-ceramic brake disc provided by the present invention optimizes the process flow and parameters, and adds a mixed powder of silicon powder, iron powder and nickel powder to perform siliconization treatment in the siliconization treatment stage. At high temperatures, iron and nickel have a catalytic graphitization effect on the resin carbon that has not been graphitized, further improving the graphitization degree of the carbon-ceramic brake disc. At the same time, after the resin carbon with higher hardness is converted into graphite, in the process of cooling after the siliconization is completed, the graphite also has the effect of hindering the expansion of cracks. The prepared sample has fewer cracks and higher strength, which can further improve the overall performance of the carbon-ceramic brake disc. In addition, the present invention adds boron compounds to the phenolic resin alcohol solution during the impregnation process, and the introduction of an appropriate amount of boron element can also promote the graphitization of the resin carbon. In the entire preparation process, no special high-temperature treatment is required to make the brake disc have a higher degree of graphitization, and low-temperature graphitization transformation is achieved. Chemical vapor deposition treatment is also not required, which can greatly save manufacturing costs. DETAILED DESCRIPTION

[0027] The embodiments described below are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] This embodiment provides a method for preparing a carbon-ceramic brake disc, and the steps for preparing the carbon-ceramic brake disc are as follows:

[0029] Step 1: preparing a carbon fiber preform of a predetermined thickness;

[0030] Step 2: impregnating the carbon fiber preform into a phenolic resin alcohol solution of a predetermined concentration, wherein the phenolic resin alcohol solution also contains a boron compound of a predetermined concentration, and forming an impregnated body after drying;

[0031] Step 3: Carbonizing the impregnated body to form a carbonized body at a carbonization temperature of 800-1100° C. for 4-6 hours;

[0032] Step 4: subjecting the carbonized body to low-temperature graphitization treatment to form a graphitized body;

[0033] Step 5: Processing the graphitized body to form a brake disc blank;

[0034] Step 6: placing the brake disc blank into a boron nitride crucible and performing siliconization treatment in a high-temperature furnace to form a silicided body, wherein the boron nitride crucible is pre-placed with filling powder, which is a mixture of silicon powder, iron powder and nickel powder;

[0035] Step 7: Processing the silicide to obtain the carbon-ceramic brake disc.

[0036] Wherein, the silicon powder content in the filling powder in step 6 is 65-90wt%, the iron powder content is 0.1-25wt% and the nickel powder content is 0.1-25wt%.

[0037] The amount of the filling powder added in step 6 is 1.1 times the mass of the brake disc blank.

[0038] The carbon fiber preform in step 1 is formed by repeatedly overlapping carbon fiber unidirectional cloth and carbon fiber mesh, and each layer of unidirectional cloth and each layer of carbon fiber mesh are stacked and needle-punched. At least one layer of carbon fiber mesh is stacked at an angle of 90° to the carbon fiber direction. The needle-punching density of the needle-punching treatment is 50-200 needles / cm2.

[0039] The concentration of the phenolic resin alcohol solution in step 2 is 40wt%.

[0040] The concentration of the boron compound in step 2 is 2-5 wt %. The boron compound can be selected from boric acid, boron oxide, boron nitride and the like.

[0041] Step 2 and step 3 are performed at least once to make the density of the carbonized body reach 1.25-1.45 g / cm3.

[0042] In step 4, the temperature of the low-temperature graphitization treatment is 1400-1800° C., and the temperature is kept for 2 hours.

[0043] The temperature of the siliconizing treatment in step 6 is 1600-1700° C., the holding time is 2-4 hours, and the pressure in the chamber of the high-temperature furnace is less than 1000 Pa.

[0044] The present invention also provides a carbon-ceramic brake disc, which contains 45-55% carbon, 40-50% silicon carbide, 8-15% silicon, 0.1-10% iron, 0.1-10% nickel and 0.5-3% boron.

[0045] Preferably, the silicon content is MSi, the total content of iron and nickel is Mm, and MSi and Mm have the following relationship:

[0046] Preferably, the graphitization degree of the carbon-ceramic brake disc is 60-95%.

[0047] Example 1

[0048] This embodiment provides a method for preparing a carbon-ceramic brake disc, and the steps for preparing the carbon-ceramic brake disc are as follows:

[0049] Step 1: Prepare a carbon fiber preform of a predetermined thickness by repeatedly overlapping carbon fiber unidirectional cloth and carbon fiber mesh tire. The carbon fiber unidirectional cloth adjacent to each layer of carbon fiber mesh tire is stacked at an angle of 90° in the direction of the carbon fiber. After each layer of unidirectional cloth and each layer of carbon fiber mesh tire are stacked, a needle punching treatment is performed. The needle punching density is 200 needles / cm 2 ;

[0050] Step 2: impregnating the carbon fiber preform into a 40wt% phenolic resin alcohol solution, adding 3wt% boric acid into the phenolic resin alcohol solution, and drying to form an impregnated body;

[0051] Step 3: The impregnated body is carbonized to form a carbonized body at a carbonization temperature of 900°C for 4 hours, and the carbonized body is impregnated and carbonized again until the density of the carbonized body reaches 1.35 g / cm 3 ;

[0052] Step 4: subjecting the carbonized body to low-temperature graphitization treatment in nitrogen at a treatment temperature of 1700° C. for 2 hours to form a graphitized body;

[0053] Step 5: Mechanically process the graphitized body to prepare the features of the product such as ventilation channels to form a brake disc blank;

[0054] Step 6: Place the brake disc blank into a boron nitride crucible and perform siliconizing treatment in a high-temperature furnace to form a silicided body, wherein the boron nitride crucible is pre-placed with a filling powder of 1.1 times the mass of the brake disc blank, wherein the silicon powder content in the filling powder is 79.9%, the iron powder is 20%, and the nickel powder is 0.1%, the siliconizing treatment temperature is 1600°C, the holding time is 3h, and the furnace pressure is less than 1000Pa;

[0055] Step 7: The silicide body is subjected to surface grinding and outer contour dimension processing to obtain the carbon ceramic brake disc.

[0056] Example 2

[0057] This embodiment provides a method for preparing a carbon-ceramic brake disc, and the steps for preparing the carbon-ceramic brake disc are as follows:

[0058] Step 1: Prepare a carbon fiber preform of a predetermined thickness by repeatedly overlapping carbon fiber unidirectional cloth and carbon fiber mesh tire. The carbon fiber unidirectional cloth adjacent to each layer of carbon fiber mesh tire is stacked at an angle of 90° in the direction of the carbon fiber. After each layer of unidirectional cloth and each layer of carbon fiber mesh tire are stacked, a needle punching treatment is performed. The needle punching density is 200 needles / cm 2 ;

[0059] Step 2: impregnating the carbon fiber preform into a 40wt% phenolic resin alcohol solution, adding 3wt% boric acid into the phenolic resin alcohol solution, and drying to form an impregnated body;

[0060] Step 3: The impregnated body is carbonized to form a carbonized body at a carbonization temperature of 900°C for 4 hours, and the carbonized body is impregnated and carbonized again until the density of the carbonized body reaches 1.35 g / cm 3 ;

[0061] Step 4: subjecting the carbonized body to low-temperature graphitization treatment in nitrogen at a treatment temperature of 1700° C. for 2 hours to form a graphitized body;

[0062] Step 5: Mechanically process the graphitized body to prepare the features of the product such as ventilation channels to form a brake disc blank;

[0063] Step 6: Place the brake disc blank into a boron nitride crucible and perform siliconizing treatment in a high-temperature furnace to form a silicided body, wherein the boron nitride crucible is pre-placed with a filling powder of 1.1 times the mass of the brake disc blank, wherein the silicon powder content in the filling powder is 78.3%, the iron powder is 0.1%, and the nickel powder is 21.6%. The siliconizing treatment temperature is 1600°C, the holding time is 3h, and the furnace pressure is less than 1000Pa;

[0064] Step 7: The silicide body is subjected to surface grinding and outer contour dimension processing to obtain the carbon ceramic brake disc.

[0065] Example 3

[0066] This embodiment provides a method for preparing a carbon-ceramic brake disc, and the steps for preparing the carbon-ceramic brake disc are as follows:

[0067] Step 1: Prepare a carbon fiber preform of a predetermined thickness by repeatedly overlapping carbon fiber unidirectional cloth and carbon fiber mesh tire. The carbon fiber unidirectional cloth adjacent to each layer of carbon fiber mesh tire is stacked at an angle of 90° in the direction of the carbon fiber. After each layer of unidirectional cloth and each layer of carbon fiber mesh tire are stacked, a needle punching treatment is performed. The needle punching density is 200 needles / cm 2 ;

[0068] Step 2: impregnating the carbon fiber preform into a 40wt% phenolic resin alcohol solution, adding 3wt% boric acid into the phenolic resin alcohol solution, and drying to form an impregnated body;

[0069] Step 3: The impregnated body is carbonized to form a carbonized body at a carbonization temperature of 900°C for 4 hours, and the carbonized body is impregnated and carbonized again until the density of the carbonized body reaches 1.35 g / cm 3 ;

[0070] Step 4: subjecting the carbonized body to low-temperature graphitization treatment in nitrogen at a treatment temperature of 1700° C. for 2 hours to form a graphitized body;

[0071] Step 5: Mechanically process the graphitized body to prepare the features of the product such as ventilation channels to form a brake disc blank;

[0072] Step 6: Place the brake disc blank into a boron nitride crucible and perform siliconizing treatment in a high-temperature furnace to form a silicided body, wherein the boron nitride crucible is pre-placed with a filling powder of 1.1 times the mass of the brake disc blank, wherein the silicon powder content of the filling powder is 91.9%, the iron powder is 10%, and the nickel powder is 0.1%, the siliconizing treatment temperature is 1600°C, the holding time is 3h, and the furnace pressure is less than 1000Pa;

[0073] Step 7: The silicide body is subjected to surface grinding and outer contour dimension processing to obtain the carbon ceramic brake disc.

[0074] Example 4

[0075] This embodiment provides a method for preparing a carbon-ceramic brake disc, and the steps for preparing the carbon-ceramic brake disc are as follows:

[0076] Step 1: Prepare a carbon fiber preform of a predetermined thickness by repeatedly overlapping carbon fiber unidirectional cloth and carbon fiber mesh tire. The carbon fiber unidirectional cloth adjacent to each layer of carbon fiber mesh tire is stacked at an angle of 90° in the direction of the carbon fiber. After each layer of unidirectional cloth and each layer of carbon fiber mesh tire are stacked, a needle punching treatment is performed. The needle punching density is 200 needles / cm 2 ;

[0077] Step 2: impregnating the carbon fiber preform into a 40wt% phenolic resin alcohol solution, adding 3wt% boric acid into the phenolic resin alcohol solution, and drying to form an impregnated body;

[0078] Step 3: The impregnated body is carbonized to form a carbonized body at a carbonization temperature of 900°C for 4 hours, and the carbonized body is impregnated and carbonized again until the density of the carbonized body reaches 1.35 g / cm 3 ;

[0079] Step 4: subjecting the carbonized body to low-temperature graphitization treatment in nitrogen at a treatment temperature of 1700° C. for 2 hours to form a graphitized body;

[0080] Step 5: Mechanically process the graphitized body to prepare the features of the product such as ventilation channels to form a brake disc blank;

[0081] Step 6: Place the brake disc blank into a boron nitride crucible and perform siliconizing treatment in a high-temperature furnace to form a silicided body, wherein the boron nitride crucible is pre-placed with a filling powder of 1.1 times the mass of the brake disc blank, wherein the silicon powder content of the filling powder is 92.4%, the iron powder is 0.1%, and the nickel powder is 7.5%, the siliconizing treatment temperature is 1600°C, the holding time is 3h, and the furnace pressure is less than 1000Pa;

[0082] Step 7: The silicide body is subjected to surface grinding and outer contour dimension processing to obtain the carbon ceramic brake disc.

[0083] Example 5

[0084] This embodiment provides a method for preparing a carbon-ceramic brake disc, and the steps for preparing the carbon-ceramic brake disc are as follows:

[0085] Step 1: Prepare a carbon fiber preform of a predetermined thickness by repeatedly overlapping carbon fiber unidirectional cloth and carbon fiber mesh tire. The carbon fiber unidirectional cloth adjacent to each layer of carbon fiber mesh tire is stacked at an angle of 90° in the direction of the carbon fiber. After each layer of unidirectional cloth and each layer of carbon fiber mesh tire are stacked, a needle punching treatment is performed. The needle punching density is 200 needles / cm 2 ;

[0086] Step 2: impregnating the carbon fiber preform into a 40wt% phenolic resin alcohol solution, adding 3wt% boric acid into the phenolic resin alcohol solution, and drying to form an impregnated body;

[0087] Step 3: The impregnated body is carbonized to form a carbonized body at a carbonization temperature of 900°C for 4 hours, and the carbonized body is impregnated and carbonized again until the density of the carbonized body reaches 1.35 g / cm 3 ;

[0088] Step 4: subjecting the carbonized body to low-temperature graphitization treatment in nitrogen at a treatment temperature of 1700° C. for 2 hours to form a graphitized body;

[0089] Step 5: Mechanically process the graphitized body to prepare the features of the product such as ventilation channels to form a brake disc blank;

[0090] Step 6: Place the brake disc blank into a boron nitride crucible and perform siliconizing treatment in a high-temperature furnace to form a silicided body. Filling powder 1.1 times the mass of the brake disc blank is pre-placed in the boron nitride crucible. The silicon powder content in the filling powder is 79.9%, the iron powder is 16.5%, and the nickel powder is 3.6%. The siliconizing treatment temperature is 1600°C, the holding time is 3h, and the furnace pressure is less than 1000Pa.

[0091] Step 7: The silicide body is subjected to surface grinding and outer contour dimension processing to obtain the carbon ceramic brake disc.

[0092] Comparative Example 1

[0093] The carbon ceramic brake disc provided in Comparative Example 1 is different from that in Example 1 in that: 1) 3 wt % of boric acid is not added to the phenolic resin alcohol solution in step 2; 2) 1.1 times the mass of the brake disc blank is pre-placed in the boron nitride crucible in step 6.

[0094] Comparative Example 2

[0095] The carbon ceramic brake disc provided in Comparative Example 1 is different from that in Example 1 in that: 1) in step 6, silicon powder 1.1 times the mass of the brake disc blank is pre-placed in the boron nitride crucible.

[0096] The carbon ceramic brake discs prepared in the above Examples 1-5 and Comparative Example 1 were tested, and the test method was as follows:

[0097] Graphitization degree test method: XRD test sample XRD spectrum, analyze the data of graphite (002) crystal surface, and calculate by the following formula

[0098] G=(0.344-d) / (0.3440-0.3354)×100%

[0099] G: degree of graphitization, %; d is the 002 crystal plane spacing, nm.

[0100] The dynamic friction coefficient and wear rate of the carbon ceramic brake disc sample were tested using the MM-1000 friction tester. The effective friction surface of the test ring has an outer diameter of D75mm / inner diameter of D55mm×10mm, and a specific pressure of 98N / cm 2 , inertia is 3kgf·cm·s 2 , linear speed is 25m / s.

[0101] The test data is shown in Table 1.

[0102] Table 1 Carbon ceramic brake disc test data of Examples 1-5 and Comparative Example 1

[0103]

[0104] It can be seen from the above examples and comparative data that by adding a mixture of different proportions of iron powder, silicon powder and nickel powder during siliconizing treatment, the graphitization degree of the carbon-ceramic brake disc can be effectively improved, the friction coefficient and the wear amount can be reduced, which is helpful to improve the service life of the carbon-ceramic brake disc. Within a certain range, the amount of iron powder added to the filling powder has a positive effect on the graphitization promotion effect of the carbon-ceramic brake disc. Within a certain range, the amount of nickel powder added to the filling powder also has a positive effect on the graphitization promotion effect of the carbon-ceramic brake disc, but the graphitization degree is always unsatisfactory. It can be seen from the data of Example 5 that the ratio between silicon powder, iron powder and nickel powder can be adjusted to achieve a better graphitization effect. The graphitization process steps of the carbon-ceramic brake disc in Comparative Example 1 saves the chemical vapor deposition and high temperature treatment steps, and there is no combined catalytic effect of the filling powder (silicon powder, iron powder and nickel powder), which leads to a decrease in the graphitization degree of the surface of the carbon-ceramic brake disc, and its wear amount is greatly increased. The quality of the carbon-ceramic brake disc is poor, and there are hidden dangers in driving safety. It can be seen from the data of Comparative Example 2 that adding boric acid to the phenolic resin alcohol solution and then impregnating the carbon fiber preform can also improve the graphitization degree of the carbon-ceramic brake disc to a certain extent.

[0105] The above disclosures are only several preferred embodiments of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. Therefore, equivalent changes made according to the scope of the patent application of the present invention are still within the scope covered by the present invention.

Claims

1. A method for preparing a carbon ceramic brake disc, characterized in that: The preparation steps of the carbon ceramic brake disc are as follows: Step 1: preparing a carbon fiber preform of a predetermined thickness; Step 2: impregnating the carbon fiber preform into a phenolic resin alcohol solution of a predetermined concentration, wherein the phenolic resin alcohol solution also contains a boron compound with a concentration of 2-5wt%, and forming an impregnated body after drying; Step 3: Carbonizing the impregnated body to form a carbonized body at a carbonization temperature of 800-1100° C. for 4-6 hours; Step 4: subjecting the carbonized body to low-temperature graphitization treatment to form a graphitized body; Step 5: Processing the graphitized body to form a brake disc blank; Step 6: placing the brake disc blank into a boron nitride crucible and performing siliconization treatment in a high-temperature furnace to form a silicided body, wherein the boron nitride crucible is pre-placed with filling powder, wherein the filling powder is a mixture of silicon powder, iron powder and nickel powder; the silicon powder content of the filling powder is 65-90wt%, the iron powder content is 0.1-25wt% and the nickel powder content is 0.1-25wt%; Step 7: Processing the silicide to obtain the carbon-ceramic brake disc.

2. The method for preparing a carbon ceramic brake disc according to claim 1, characterized in that: The added amount of the filling powder is 1.1 times the mass of the brake disc blank.

3. The method for preparing a carbon ceramic brake disc according to claim 1, characterized in that: The carbon fiber preform is formed by repeatedly overlapping carbon fiber unidirectional cloth and carbon fiber mesh, and each layer of unidirectional cloth and each layer of carbon fiber mesh are needle-punched after being overlapped.

4. The method for preparing a carbon ceramic brake disc according to claim 3, characterized in that: At least one layer of carbon fiber web tire has upper and lower adjacent carbon fiber unidirectional fabrics stacked at an angle of 90 degrees in the direction of the carbon fibers.

5. The method for preparing a carbon ceramic brake disc according to claim 3, characterized in that: The needle density of the needle treatment is 50-200 needles / cm 2 .

6. The method for preparing a carbon ceramic brake disc according to claim 1, characterized in that: The concentration of the phenolic resin alcohol solution in step 2 is 40wt%.

7. The method for preparing a carbon ceramic brake disc according to claim 1, characterized in that: Step 2 and step 3 are performed at least once, so that the density of the carbide reaches 1.25-1.45 g / cm 3 .

8. The method for preparing a carbon ceramic brake disc according to claim 1, characterized in that: In step 4, the temperature of the low-temperature graphitization treatment is 1400-1800° C., and the temperature is kept for 2 hours.

9. The method for preparing a carbon ceramic brake disc according to claim 1, characterized in that: The temperature of the siliconizing treatment in step 6 is 1600-1700° C., the holding time is 2-4 hours, and the pressure in the chamber of the high-temperature furnace is less than 1000 Pa.

10. A carbon-ceramic brake disc made by the method for making a carbon-ceramic brake disc according to any one of claims 1 to 9, characterized in that: The carbon ceramic brake disc contains 45-55% carbon, 40-50% silicon carbide, 8-15% silicon, 0.1-10% iron, 0.1-10% nickel and 0.5-3% boron.

11. The carbon-ceramic brake disc according to claim 10, characterized in that: The silicon content is M Si , the total content of iron and nickel is M m , M Si and M m With the following relationship:

12. The carbon-ceramic brake disc according to claim 10, characterized in that: The graphitization degree of the carbon ceramic brake disc is 60-95%.

Citation Information

Patent Citations

  • Carbon-fiber composite material for skis of magnetic suspension train

    CN1631845A

  • Graphite material

    WO2018115177A1

Cited By

  • Method for preparing carbon-ceramic brake disc from carbon / ceramic-based composite material

    CN120736914A