Method for purifying selenium, germanium, gallium, and barium polycrystalline materials and growing high-transmittance crystals by horizontal gradient crystallization

The selenium, germanium, gallium and barium polycrystalline material was purified by the horizontal gradient crystallization method and the vertical Bridgman single crystal growth method was used to solve the problem of low purity of the BaGa2GeSe6 polycrystal and achieve high transmittance BGGSe single crystal growth, which is suitable for infrared radiation. Applications of power solid-state lasers.

CN117867649BActive Publication Date: 2024-10-18HARBIN INST OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410111972.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-26
Publication Date
2024-10-18
Estimated Expiration
2044-01-26

AI Technical Summary

Technical Problem

The BaGa2GeSe6 polycrystal synthesized by existing methods has low purity, which affects the transmittance performance of the single crystal and limits its application in infrared high-power solid-state lasers.

Method used

The horizontal gradient crystallization method is used to purify selenium, germanium, gallium and barium polycrystalline materials, and high-transmittance BGGSe single crystals are grown in a vertical Bridgman single crystal growth furnace. By controlling the temperature gradient and chemical reaction conditions, the purity of the polycrystalline materials is improved. and single crystal transmittance.

Benefits of technology

The transmittance of the BaGa2GeSe6 single crystal is significantly improved, ensuring that the transmittance in the range of 0.6 to 17 μm is greater than 55%. It is suitable for the optical field, especially in applications in the 10 to 14 μm band.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117867649B_ABST
    Figure CN117867649B_ABST
Patent Text Reader

Abstract

The invention discloses a method for purifying a polycrystalline material of selenium, germanium, gallium, and barium and growing a high-transmittance crystal by a horizontal gradient crystallization method, and relates to a method for purifying a polycrystalline material of selenium, germanium, gallium, and barium and growing a single crystal. The method aims to solve the technical problem that the BaGa2GeSe6 polycrystalline synthesized by the existing method has low purity, which in turn affects the transmittance of the single crystal. The method comprises the following steps: firstly weighing a Ba source, a Ga source, a Ge source, and a Se source according to the stoichiometric ratio of BaGa2GeSe6 and placing them in a crucible, and then placing them in a quartz tube, evacuating and melting and sealing them; placing them in a horizontal tube furnace and carrying out polycrystalline synthesis through a reaction stage, a homogenization stage, and a gradient crystallization stage; and then crushing them and growing a BGGSe single crystal in a vertical Bridgman single crystal growth furnace. The transmittance of the single crystal grown by the invention is greater than 55% in a wide range of 0.6 to 17 μm. The method can be used in the field of nonlinear optical frequency conversion technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for purifying selenium, germanium, gallium and barium polycrystalline materials and growing single crystals. Background Art

[0002] The synthesis process of nonlinear optical crystals (such as LBO, BBO and KBBF) in the ultraviolet and visible light bands is relatively mature, but the intrinsic defects of chalcopyrite crystals (such as AgGaS2, AgGaSe2 and ZnGeP2) for commercial applications in the infrared band, such as low laser damage threshold and two-photon absorption, limit their application in far-infrared high-power solid-state lasers. The development of modern infrared laser technology requires new crystals with the following properties: First, they can efficiently utilize the 1064nm laser pump output by Nd:YAG lasers. Secondly, the new crystal needs to cover an output range of more than 10μm, especially the 10-14μm range is the radiation peak band of low-temperature targets, suitable for photoelectric countermeasures, and there are many fingerprint areas of molecular vibration in this band.

[0003] Compared with other infrared nonlinear optical crystals, BGGSe has advantages in device processing in that its surface chemical properties are stable, no post-growth treatment is required, and the crystal has high symmetry. Due to the low dispersion properties and high damage threshold of BGGSe crystal, it has advantages in ultra-wide frequency mixing and ultra-short pulse output.

[0004] The Chinese patent application number 201110174671.6, "Nonlinear optical crystal gallium germanium barium selenide and its growth method and use", discloses the use of a solid phase synthesis method to sinter at high temperature to obtain a BaGa2GeSe6 compound. The crucible descent method is used to grow a BGGSe single crystal. However, the purity of the BaGa2GeSe6 polycrystal obtained by this method is low, which affects the transmittance performance of the subsequently grown single crystal. Summary of the invention

[0005] The present invention aims to solve the technical problem that the BaGa2GeSe6 polycrystals synthesized by the existing method have low purity, which in turn affects the transmittance of the single crystal, and provides a method for purifying the selenium-germanium-gallium-barium polycrystal material and growing high-transmittance crystals by a horizontal gradient crystallization method.

[0006] The method for purifying selenium, germanium, gallium, and barium polycrystalline materials and growing high-transmittance crystals by a horizontal gradient crystallization method of the present invention is carried out according to the following steps:

[0007] 1. In an inert atmosphere glove box, weigh Ba source, Ga source, Ge source and Se source according to the stoichiometric ratio of BaGa2GeSe6; place the weighed raw materials in a crucible, then place the crucible in a quartz tube, and add 0.01 to 20.00 g of elemental Se to the quartz tube, evacuate to a vacuum state using a molecular pump, then fill the quartz tube with inert gas until the reading of the external pressure vacuum gauge reaches -0.010 to -0.015 MPa, and then use a hydrogen-oxygen flame to melt and seal;

[0008] 2. Place the sealed quartz tube into a horizontal tube furnace, with the mixture of barium, gallium and germanium in the high temperature zone and selenium in the low temperature zone, to perform polycrystalline synthesis, specifically:

[0009] (1) Reaction stage: In order to better suppress the intensity of the chemical reaction, the high temperature zone is heated to 650-850°C at a rate of 5-20°C / h and kept at this temperature for 5-20 hours. The purpose of this process is to control the reaction rate of the active metal barium and the non-metallic selenium element to avoid the violent reaction causing the final product of the compound to deviate from the stoichiometric ratio; after keeping warm, the temperature is continued to be raised to 950-1050°C at a rate of 5-10°C / h and kept at this temperature for 10-30 hours. The purpose is to completely melt the high melting point metal germanium to ensure the complete selenization reaction; in this stage, the low temperature zone is heated to 700°C at a rate of 5-20°C / h and kept at 700°C throughout the process;

[0010] (2) Homogenization stage: After the reaction stage is completed, the temperature field in the low temperature zone is rapidly heated to 1050-1100°C at a rate of 10-30°C / h, and the temperature field in the high temperature zone is kept at 950-1050°C for 50-60h; the purpose of this stage is to promote the complete reaction of the binary and ternary selenides formed in the crucible in the high temperature zone to form a homogenized BGGSe single homogeneous compound;

[0011] (3) Gradient crystallization stage: the temperature field is changed rapidly at a rate of 20 to 50°C / h, a temperature field with a gradient of 1 to 5°C / cm is formed in the high temperature zone, and gradient crystallization is performed at a rate of 0.1 to 10 mm / h. After gradient crystallization for 200 mm, the temperature is reduced to 750°C at a rate of 3 to 7°C / h and then kept at this temperature for 10 to 30 hours, and then reduced to room temperature at a rate of 15 to 30°C / h. During this process, the low temperature zone maintains a cooling rate of 30 to 40°C / h. The purpose is to allow the additional substances (Se, P, I, GeSe2, etc.) used to provide atmosphere pressure to settle in the low temperature section to avoid settling inside the crucible, which causes the obtained BaGa2GeSe6 compound to deviate from the stoichiometric ratio; and obtain a polycrystalline BaGa2GeSe6 compound;

[0012] 3. After taking out the BaGa2GeSe6 compound polycrystalline material, crush it in a mortar, put it in a PBN crucible, and then put the PBN crucible in a quartz tube. Add 0.1-5.0g of Se element to the quartz tube to provide Se vapor atmosphere, and then use a molecular pump to evacuate to 10 -5 Pa, melt-sealed with the aid of hydrogen-oxygen flame;

[0013] 4. Place the sealed quartz tube in a vertical Bridgman single crystal growth furnace, wherein the powdered BGGSe polycrystalline material is placed in a constant temperature zone 20 to 50°C higher than the melting point of the polycrystalline material. After keeping the temperature for 20 to 100 hours, single crystal growth is carried out, the temperature gradient is 5 to 20°C / cm, and the growth rate is 0.1 to 2.0 mm / h. After the growth is completed, the temperature is lowered to room temperature at a rate of 5 to 60°C / h to obtain a BGGSe single crystal, which is a red and transparent crystal.

[0014] Furthermore, the Ba source in step 1 is bulk metal elemental barium, powdered metal elemental barium, beaded metal elemental barium or barium selenide compound (BaSe);

[0015] Furthermore, the Ga source in step 1 is bulk metal single substance gallium, liquid metal single substance gallium, bead metal single substance gallium or gallium triselenide (Ga2Se3);

[0016] Furthermore, the Ge source in step 1 is bulk single crystal germanium, powdered metallic germanium, beaded metallic germanium or germanium diselenide (GeSe2);

[0017] Furthermore, the Se source in step 1 is powdered elemental selenium, beaded elemental selenium, barium selenide (BaSe), gallium triselenide (Ga2Se3) or germanium diselenide (GeSe2).

[0018] Furthermore, the inert atmosphere described in step 1 refers to N2, Ar or He atmosphere.

[0019] Furthermore, the inert gas described in step 1 refers to N2, Ar or He gas.

[0020] Furthermore, the built-in cylindrical crucible described in step 2 is a carbon-coated quartz crucible, a high-purity corundum crucible, a high-purity graphite crucible or a high-purity pyrolytic boron nitride crucible.

[0021] Furthermore, the vacuum state described in step 1 is that the pressure in the tube is evacuated to 10 -4 Below Pa.

[0022] The present invention further purifies the high-purity selenium-germanium-gallium-barium polycrystalline material synthesized in two temperature zones by means of gradient crystallization, so that the purity of the area with better crystallinity is significantly improved, wherein the ternary phase impurities are removed to the tail by means of horizontal gradient crystallization, and the use of the material in the area with better crystallinity for single crystal growth is conducive to improving the transmittance of the grown single crystal, and the transmittance of the single crystal of the present invention is greater than 55% in a wide range of 0.6 to 17 μm. It can be used in the optical field. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 1 is a schematic structural diagram of the vertical Bridgman single crystal growth furnace in Example 1; in the figure, 1 is an aluminum cavity, 2 is a cover, 3 is a heating tube, 4 is a moving platform, 5 is a first temperature measuring device, 6 is a second temperature measuring device, 7 is a low temperature zone, 8 is a crystallization zone, 9 is a high temperature zone, 10 is a PBN crucible, 11 is a quartz tube, 12 is a crystal, and 13 is a melt;

[0024] Figure 2 is a temperature field temperature curve diagram during single crystal growth in Example 1;

[0025] Figure 3 The photo of the BaGa2GeSe6 compound polycrystalline material obtained in step 2 of Example 1 and the XRD spectra of the corresponding regions;

[0026] Figure 4 is a photograph of the single crystal obtained in step 4 of Example 1;

[0027] Figure 5 is a transmittance curve diagram of a single crystal obtained in step 4 of Example 1;

[0028] Figure 6 This is the EDS spectrum of the single crystal obtained in step 4 of Example 1. DETAILED DESCRIPTION

[0029] The beneficial effects of the present invention are verified by the following examples.

[0030] Embodiment 1: The method of purifying the polycrystalline material of selenium, germanium, gallium and barium and growing high-transmittance crystals by the horizontal gradient crystallization method of this embodiment is carried out according to the following steps:

[0031] 1. In a glove box with an Ar gas atmosphere, 30.228 g of powdered metal element barium (Ba), 30.682 g of bulk metal element gallium (Ga), 16.224 g of powdered metal element germanium (Ge) and 103.81 g of powdered element selenium (Se) were weighed, i.e., Ba:Ga:Ge:Se=0.11 mol:0.22 mol:0.11 mol:0.66 mol; the weighed barium, gallium and germanium were mixed and placed in a boat-shaped PBN crucible, the mixture of barium, gallium and germanium was placed at one end of the boat-shaped PBN crucible, the weighed selenium was placed in another boat-shaped PBN crucible, and the two boat-shaped PBN crucibles were placed at both ends of a horizontal quartz tube with a diameter of 45 mm, and 10.00 g of elemental Se was additionally added to the quartz tube, and the pressure in the quartz tube was pumped to 10 -4 Pa, and then fill the quartz tube with Ar gas until the reading of the external pressure vacuum gauge reaches -0.010MPa, which is used to increase the pressure in the tube and reduce the deviation of the synthetic product from the stoichiometric ratio caused by the escape of compounds at high temperature, and then use hydrogen-oxygen flame to melt and seal the quartz tube;

[0032] 2. Place the sealed quartz tube into an eight-temperature-zone horizontal tube furnace, with the mixture of barium, gallium and germanium in the high-temperature zone and selenium in the low-temperature zone for polycrystalline synthesis, specifically:

[0033] (1) Reaction stage: In order to better suppress the intensity of the chemical reaction, the high temperature zone is heated to 750°C at a rate of 20°C / h and kept at this temperature for 10 hours. The purpose of this process is to control the reaction rate of the active metal barium and the non-metallic selenium element to avoid the violent reaction causing the final product of the compound to deviate from the stoichiometric ratio; after keeping warm, the temperature is continued to be raised to 1020°C at a rate of 10°C / h and kept at this temperature for 20 hours. The purpose is to completely melt the high-melting-point metal germanium to ensure the complete selenization reaction; in this stage, the low temperature zone is heated to 700°C at a rate of 20°C / h and kept at 700°C throughout the process;

[0034] (2) Homogenization stage: After the reaction stage is completed, the temperature field in the low temperature zone is rapidly heated to 1050°C at a rate of 20°C / h, and the temperature field in the high temperature zone is kept at 1020°C for 60 hours; the purpose of this stage is to promote the complete reaction of the binary and ternary selenides formed in the crucible in the high temperature zone to form a homogenized BGGSe single homogeneous compound;

[0035] (3) Gradient crystallization stage: the temperature field is changed rapidly at a rate of 30°C / h, a temperature field with a gradient of 3°C / cm is formed in the high temperature zone, and gradient crystallization is performed at a rate of 0.1mm / h. After gradient crystallization for 200mm, the temperature is reduced to 750°C at a rate of 5°C / h and then kept at this temperature for 24h, and then reduced to room temperature at a rate of 25°C / h. During this process, the low temperature zone maintains a cooling rate of 30°C / h, the purpose of which is to allow the additional material used to provide the atmosphere pressure to settle in the low temperature section, and avoid settling inside the crucible, which causes the obtained BaGa2GeSe6 compound to deviate from the stoichiometric ratio; and obtain a polycrystalline BaGa2GeSe6 compound;

[0036] 3. After taking out the polycrystalline BaGa2GeSe6 compound with good crystallinity, crush it in a mortar until the particle size is less than 2 mm, then put 100 g of polycrystalline powder into a PBN crucible, and then put the PBN crucible into a quartz tube with a diameter of 40 mm, and add 2.153 g of Se elemental substance to the quartz tube to provide Se vapor atmosphere, and then use a molecular pump to evacuate to 10 -5 Pa, melt-sealed with the aid of hydrogen-oxygen flame;

[0037] 4. Place the sealed quartz tube in a vertical Bridgman single crystal growth furnace, wherein the vertical Bridgman single crystal growth furnace consists of an aluminum cavity 1, a cover 2, a heating tube 3, and a moving platform 4; the cover 2 is arranged at the upper end of the aluminum cavity 1, the moving platform 4 is arranged at the lower part of the aluminum cavity 1, the heating tube 3 is wrapped around the outside of the aluminum cavity 1, and a first temperature measuring device 5 and a second temperature measuring device 6 are respectively arranged in the middle section and the lower section of the aluminum cavity 1, and the aluminum cavity 1 forms a low temperature zone 7, a crystallization zone 8 and a high temperature zone 9 from bottom to top; place a quartz tube 11 equipped with a PBN crucible 10 in a vertical Bridgman single crystal growth furnace, wherein the powdered BGGSe polycrystalline material in the PBN crucible 10 is located in a constant temperature zone 30°C higher than the melting point of the polycrystalline material, and single crystal growth is carried out after keeping warm for 50 hours, the temperature gradient is 5°C / cm, the growth rate is 0.1mm / h, and after the growth is completed, it is cooled to room temperature at a rate of 20°C / h. The temperature field temperature curve during the single crystal growth is as shown in Figure 2 As shown, a BGGSe single crystal is obtained, which is a red and transparent crystal.

[0038] The BaGa2GeSe6 compound polycrystalline material obtained in step 2 of this embodiment has a crystal length of 200 mm. Figure 3 As shown in b, the polycrystalline material is divided into five regions along the length direction, namely S1, S2, S3, S4 and S5, and samples are taken from each region to test the XRD spectrum, as shown in FIG. Figure 3 As shown in a, from Figure 3 It can be seen that the purity of the S1, S2, and S3 regions with better crystallinity is significantly improved, and the ternary phase impurities are removed to the S4 and S5 regions at the tail through horizontal gradient crystallization.

[0039] In this embodiment, a single crystal is grown by vertical Bridgman crucible descent method under the condition of temperature gradient of 20°C / cm. The obtained single crystal is cut into wafers with length, width and thickness of 9mm×5mm×5mm and double-sided polishing is performed. The photo of the transparent wafer is shown in FIG. Figure 4 As shown, the transmittance curve of the chip is as follows Figure 5 As shown, from Figure 5 It can be seen that the high transmittance of more than 55% can be maintained within a wide range of 0.6 to 17 μm.

[0040] The element distribution map obtained by scanning the grown BaGa2GeSe6 single crystal region using an energy dispersive X-ray spectrometer (EDS) is shown in the figure. Figure 6 As shown, from Figure 6 It can be seen that the Ba, Ga, Ge and Se elements are evenly distributed in the transparent wafer.

Claims

1. A method for purifying selenium, germanium, gallium and barium polycrystalline materials and growing high-transmittance crystals by horizontal gradient crystallization, characterized in that: The method proceeds as follows:

1. In an inert atmosphere glove box, weigh Ba source, Ga source, Ge source and Se source according to the stoichiometric ratio of BaGa2GeSe6; place the weighed raw materials in a crucible, then place the crucible in a quartz tube, and add 0.01~20.00g of elemental Se to the quartz tube, use a molecular pump to evacuate to a vacuum state, then fill the quartz tube with inert gas until the reading of the external pressure vacuum gauge reaches -0.010~-0.015MPa, and then use a hydrogen-oxygen flame to melt and seal; 2. Place the sealed quartz tube in a horizontal tube furnace, with the mixture of barium, gallium and germanium in the high temperature zone and selenium in the low temperature zone, to perform polycrystalline synthesis, specifically: Reaction stage: the high temperature zone is heated to 650-850°C at a rate of 5-20°C / h and kept at this temperature for 5-20 hours; after keeping at this temperature, the temperature is further heated to 950-1050°C at a rate of 5-10°C / h and kept at this temperature for 10-30 hours; during this stage, the low temperature zone is heated to 700°C at a rate of 5-20°C / h and kept at 700°C throughout the process; Homogenization stage: After the reaction stage is completed, the temperature field in the low temperature zone is rapidly heated to 1050~1100 ℃ at a rate of 10~30 ℃ / h, and the temperature field in the high temperature zone is kept at 950~1050 ℃ for 50~60h; Gradient crystallization stage: the temperature field is changed rapidly at a rate of 20-50 °C / h, a temperature field with a gradient of 1-5 °C / cm is formed in the high temperature zone, and gradient crystallization is performed at a rate of 0.1-10 mm / h. After gradient crystallization for 200 mm, the temperature is reduced to 750 °C at a rate of 3-7 °C / h and then kept at this temperature for 10-30 hours, and then reduced to room temperature at a rate of 15-30 °C / h. During this process, the low temperature zone maintains a cooling rate of 30-40 °C / h; 3. After taking out the polycrystalline material of BaGa2GeSe6 compound, crush the polycrystalline material with good crystallinity in a mortar, put it into a PBN crucible, and then put the PBN crucible into a quartz tube. Add 0.1-5.0 g of Se element to the quartz tube to provide Se vapor atmosphere, and then use a molecular pump to evacuate to 10 -5 Pa, melt-sealed with the aid of hydrogen-oxygen flame; 4. Place the sealed quartz tube in a vertical Bridgman single crystal growth furnace, in which the powdered BGGSe polycrystalline material is placed in a constant temperature zone 20~50 ℃ higher than the melting point of the polycrystalline material. After keeping warm for 20~100 h, single crystal growth is carried out with a temperature gradient of 5~20 ℃ / cm and a growth rate of 0.1~2.0 mm / h. After the growth is completed, the temperature is lowered to room temperature at a rate of 5~60 ℃ / h to obtain a BGGSe single crystal.

2. The method for purifying selenium, germanium, gallium, and barium polycrystalline materials and growing high-transmittance crystals by horizontal gradient crystallization according to claim 1, characterized in that: The Ba source described in step 1 is bulk metal elemental barium, powdered metal elemental barium, beaded metal elemental barium or barium selenide.

3. The method for purifying selenium, germanium, gallium, and barium polycrystalline materials and growing high-transmittance crystals by horizontal gradient crystallization according to claim 1 or 2, characterized in that: The Ga source described in step 1 is bulk metal single substance gallium, liquid metal single substance gallium, bead metal single substance gallium or gallium triselenide.

4. The method for purifying selenium, germanium, gallium, and barium polycrystalline materials and growing high-transmittance crystals by horizontal gradient crystallization according to claim 1 or 2, characterized in that: The Ge source described in step 1 is bulk single crystal germanium, powdered metallic germanium, beaded metallic germanium or germanium diselenide.

5. The method for purifying selenium, germanium, gallium, and barium polycrystalline materials and growing high-transmittance crystals by horizontal gradient crystallization according to claim 1 or 2, characterized in that: The Se source described in step 1 is powdered elemental selenium, beaded elemental selenium, barium selenide, gallium triselenide or germanium diselenide.

6. The method for purifying selenium, germanium, gallium, and barium polycrystalline materials and growing high-transmittance crystals by horizontal gradient crystallization according to claim 1 or 2, characterized in that: The inert atmosphere described in step 1 refers to N2, Ar or He atmosphere.

7. The method for purifying selenium, germanium, gallium, and barium polycrystalline materials and growing high-transmittance crystals by horizontal gradient crystallization according to claim 1 or 2, characterized in that: The vacuum state described in step 1 is that the pressure in the tube is evacuated to 10 -4 Below Pa.

Citation Information

Patent Citations

  • Nonlinear optical crystal gallium germanium barium selenide as well as growing method and purposes thereof