A crack-resistant ceramic rock plate and its paving process

By adding silicon nitride whiskers to ceramic rock slabs and using silicone water-based polyurethane adhesives, the problems of low crack resistance and pollution in the paving process of ceramic rock slabs have been solved, and an efficient and environmentally friendly paving process has been achieved, improving It improves the crack resistance and paving efficiency of ceramic rock slabs.

CN117886587BActive Publication Date: 2024-10-11DONGGUAN COHUI IND MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410069003.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-17
Publication Date
2024-10-11
Estimated Expiration
2044-01-17

AI Technical Summary

Technical Problem

Traditional ceramic slates have low crack resistance during processing and use, and the mortar or tile adhesive used in traditional paving processes leads to increased building weight, serious environmental pollution, and bonding failure, causing ceramic slates to fall off.

Method used

By optimizing the raw materials of ceramic rock slabs, adding silicon nitride whiskers to toughen them, and synthesizing a silicone water-based polyurethane adhesive with good stability and water resistance, using 'thin coating technology' for paving, simplifying the paving process and reducing adhesion. Layer thickness and weight.

Benefits of technology

It improves the crack resistance of ceramic rock slabs, simplifies the paving process, reduces material and energy consumption, reduces environmental pollution and carbon emissions, and achieves the goals of lightweight and low labor intensity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004669260700000031
    Figure BDA0004669260700000031
  • Figure BDA0004669260700000071
    Figure BDA0004669260700000071
  • Figure BDA0004669260700000111
    Figure BDA0004669260700000111
Patent Text Reader

Abstract

The invention relates to the technical field of interior decoration, and discloses a crack-resistant ceramic rock board and a paving process thereof. The synthesized sodium dihydroxysiloxane benzene sulfonate monomer contains a hydroxyl group, an ether bond, an amine bond and the like with relatively large polarity, and the sodium sulfonate in the structure thereof has strong hydrophilicity, so that the polyurethane dispersion has more stable performance. Meanwhile, the organic silicone waterborne polyurethane adhesive contains more Si-O-Si structures and has lower surface tension, so that the prepared adhesive has better storage stability and good water resistance. The silicon nitride whisker has good interface bonding with the ceramic phase and has good physical and chemical compatibility. Under the action of external loads, the whisker can be partially digested and dispersed to a certain extent, so as to enhance the crack resistance of the ceramic rock board. The paving process of the invention can realize ultra-thin paving, simplify the paving process of the ceramic rock board, and conform to the environmental protection concept of energy saving and emission reduction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of interior decoration, and in particular to a crack-resistant ceramic rock slab and a paving process thereof. Background Art

[0002] With the changes in application scenarios in the new era, heavy ceramic slabs can no longer meet consumers' personalized decoration needs, so the "thin revolution" of traditional ceramic slabs is also imminent; ceramic rock slabs are a kind of plate-shaped ceramic products made of kaolin clay and other inorganic non-metallic materials through molding, high-temperature calcination and other production processes. While ensuring the product's function, the product's thinness is maximized, and the product thickness is less than 6mm; compared with similar products, the amount of building ceramic materials per unit area is reduced by more than half, saving more than 60% of raw material resources and reducing comprehensive energy consumption by more than 50%. Whether from the amount of raw materials used or the energy consumption in the production process, it can well achieve the low-carbon goal of "saving materials and energy"; for product users, thin and lightweight large-size panels not only save logistics and transportation costs, reduce the load of buildings, but also directly reduce the carbon emissions of logistics and construction; however, large-size ultra-thin porcelain tiles have many technical difficulties in processing and use due to their large area and thin thickness, among which the problem of low crack resistance is particularly prominent.

[0003] Traditional paving technology generally uses mortar or tile adhesive for construction, and the thickness of the bonding layer is generally 0.5-3mm. The mortar or tile adhesive has a high specific gravity and a large workload. It will not only increase the weight of the building, but also cause deformation and dislocation of the cement slurry on the back of the tile, resulting in a layer of extremely water-rich mortar layer between the tile and the slurry, which will cause "hollowing" after drying. Moreover, the cement used in tile adhesive and mortar is a high-energy consumption and highly polluting product, which poses a serious threat to the environment. Analysis of the new ceramic wall and floor tile pasting process Compared with the traditional process, the main difference between the new ceramic wall and floor tile adhesive pasting process lies in the application method and thickness of the adhesive. However, the existing adhesive is not stable enough and has poor water resistance, which makes the bonding between the ceramic rock slab and the base fail, and then falls off. Therefore, it is of great significance to prepare an adhesive with stable dispersion and water resistance to broaden the application of ceramic rock slabs.

[0004] The present invention optimizes the raw materials of ceramic rock slabs and adds silicon nitride whiskers for toughening and strengthening, so that the prepared ceramic rock slabs have better crack resistance, and at the same time synthesizes a silicone water-based polyurethane adhesive with good stability and water resistance, and adopts "thin coating technology" for paving, which simplifies the paving process of ceramic rock slabs and complies with the environmental protection concept of energy saving and emission reduction. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a crack-resistant ceramic rock slab and its paving process, thereby improving the crack resistance of the ceramic rock slab and simplifying the paving process of the ceramic rock slab.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A crack-resistant ceramic rock plate comprises the following components in parts by weight: 20-46 parts of kaolin, 15-25 parts of quartz, 5-10 parts of high-white sodium feldspar, 4-8 parts of wollastonite, 3-12 parts of potassium feldspar, 5-15 parts of spodumene, and 2-10 parts of silicon nitride whiskers; the preparation method of the crack-resistant ceramic rock plate comprises the following steps: adding kaolin, quartz, high-white sodium feldspar, potassium feldspar, spodumene, wollastonite, and silicon nitride whiskers into a ball mill, ball-milling the mixture, passing through a 200-300 mesh sieve, adding 10-30 parts of deionized water for granulation, pressing and forming with an electric hydraulic brick machine, transferring to a silicon carbon rod furnace, sintering, and naturally cooling to obtain the crack-resistant ceramic rock plate.

[0008] Preferably, the sintering temperature is 1000-1200° C., the sintering time is 3-5 hours, and the heating rate is 5-8° C. / min.

[0009] Preferably, the steps are included: before construction, check and clean the base layer, the height error is between 0.1-3mm, and the silicone water-based polyurethane adhesive is evenly applied to the upper surface of the base layer with the serrated edge of a plastering knife. The thickness of the adhesive layer is 1-5mm. After the adhesive and the base layer are fully infiltrated, the surface of the anti-cracking ceramic rock board is polished with sandpaper. After cleaning and drying, the adhesive is applied to the lower surface of the anti-cracking ceramic rock board with the straight edge of a plastering knife. A layer is then applied, and the applied anti-cracking ceramic rock board is then pasted to the upper surface of the base layer coated with the silicone water-based polyurethane adhesive, and a vibrator is used for leveling and compacting.

[0010] Preferably, the plastering tooth knife is a V-shaped plastering tooth knife or a U-shaped plastering tooth knife, and the tooth depth is 1-8mm.

[0011] Preferably, the preparation method of the silicone waterborne polyurethane adhesive comprises the following steps:

[0012] (1) Add 1,1,3,3-tetramethyl-1,3-bis[3-(oxiranylmethoxy)propyl]disiloxane and N,N-dimethylformamide to a reaction flask, mix well, add sodium p-aminobenzenesulfonate, stir to react, concentrate after the reaction is completed, and recrystallize the product in an ethanol aqueous solution to obtain a sodium bishydroxysiloxane benzenesulfonate monomer. The preparation process is as follows:

[0013]

[0014] (2) In a four-necked flask equipped with a thermometer, a condenser reflux tube and a stirrer, polytetramethylene glycol, isophorone diisocyanate and a catalyst dibutyltin dilaurate are added, and the mixture is stirred at 70-80° C. for 2-3 hours. Then, sodium dihydroxysiloxane benzenesulfonate monomer is added and the reaction is carried out for 1-1.5 hours. Then, KH550 is added for end-capping. The reaction system is cooled to 30° C., and deionized water is slowly added to the system. The mixture is stirred and emulsified to obtain a silicone waterborne polyurethane adhesive.

[0015] Preferably, in the step (1), the amount of 1,1,3,3-tetramethyl-1,3-bis[3-(oxiranylmethoxy)propyl]disiloxane is 100 parts by weight and the amount of sodium p-aminobenzenesulfonate is 115-160 parts by weight.

[0016] Preferably, in step (1), the reaction temperature is 55-70° C. and the reaction time is 8-16 h.

[0017] Preferably, in the step (2), by weight, polytetramethylene glycol is 100 parts, isophorone diisocyanate is 28-35 parts, dibutyltin dilaurate is 0.8-1.5 parts, sodium bishydroxysiloxane benzenesulfonate monomer is 32-40 parts, and KH550 is 1-5 parts.

[0018] By adopting the above technical solution, the beneficial effects of the present invention are:

[0019] The present invention firstly allows the epoxy of 1,1,3,3-tetramethyl-1,3-bis[3-(oxiranylmethoxy)propyl]disiloxane to undergo a ring-opening reaction with the amino group of sodium p-aminobenzenesulfonate to obtain a sodium bishydroxysiloxane benzenesulfonate monomer, then adds the sodium bishydroxysiloxane benzenesulfonate monomer as a chain extender into a mixed system of polytetramethylene ether glycol and isophorone diisocyanate, and then uses KH550 as a capping agent to obtain an organic silicone waterborne polyurethane adhesive; then uses kaolin, quartz, albite and the like as raw materials, adds silicon nitride whiskers for toughening, and obtains a crack-resistant ceramic rock slab after ball milling, pressing and sintering; finally, a "thin coating technology" is used for paving, which simplifies the paving process of the ceramic rock slab and meets the environmental protection concept of energy saving and emission reduction.

[0020] The synthesized sodium bishydroxysiloxane benzene sulfonate monomer of the present invention contains hydroxyl groups, ether bonds, amine bonds, etc. with relatively large polarity, which endow the adhesive with high bonding strength, cohesive strength and chemical stability. The sodium sulfonate in the structure has strong hydrophilicity, so that the polyurethane dispersion has a more stable "double electric layer" structure and has better compatibility with the waterborne polyurethane adhesive system. At the same time, the sodium bishydroxysiloxane benzene sulfonate monomer contains a Si-O-Si structure and has a relatively low surface tension, so that the surface energy of the system is reduced. In the film-forming stage of the polyurethane adhesive, the hydrophobic organic silicon segment migrates to the surface of the polyurethane adhesive. The silicon nitride whiskers are introduced into the ceramic phase, which has good physical and chemical compatibility with the ceramic phase, and the interface bonding between the two is good, thereby forming a reinforcing phase in the ceramic phase. Therefore, under the action of external loads, the whiskers can be partially dissolved and dispersed to a certain extent, and the crack propagation path is effectively extended, so that more energy is required for the sample to break, thereby enhancing the fracture strength of the ceramic rock plate and making it have better crack resistance.

[0021] The paving process of the present invention can achieve ultra-thin paving, the thickness of the bonding layer can be reduced by up to 80%, the weight is greatly reduced, the ceramic rock slab paving process is simplified, and the paving does not require the use of heavy polluting products such as cement sand, thereby achieving the goal of lightweight and low labor intensity; the paving process of the present invention complies with the environmental protection concept of energy saving and emission reduction from aspects such as bonding layer thickness, material density, construction efficiency, transportation cost and materials to energy consumption in the production and construction process, and greatly reduces carbon emissions; this process has achieved high social value in terms of energy saving and emission reduction, aging transformation, installation renovation, demolition-free renovation, reducing construction waste, and reducing building weight. DETAILED DESCRIPTION

[0022] In order to more clearly illustrate the present invention and have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.

[0023] Example 1

[0024] (1) Add 10 parts by weight of 1,1,3,3-tetramethyl-1,3-bis[3-(oxiranylmethoxy)propyl]disiloxane and 180 mL of N,N-dimethylformamide to a reaction flask, mix well, add 15 parts of sodium p-aminobenzenesulfonate, react at 60° C. for 12 h, concentrate, and recrystallize the product in a 75% by volume ethanol aqueous solution to obtain a sodium bishydroxysiloxane benzenesulfonate monomer.

[0025] (2) In a four-necked flask equipped with a thermometer, a condenser reflux tube and a stirrer, 100 parts of polytetramethylene glycol (molecular weight 2000), 30 parts of isophorone diisocyanate and 1.2 parts of catalyst dibutyltin dilaurate were added by weight, stirred at 75°C for 3 hours, and then 32 parts of sodium bishydroxysiloxane benzenesulfonate monomer were added and reacted for 1 hour. Then, 1 part of KH550 was added for end-capping, the reaction system was cooled to 30°C, and deionized water was slowly added to the system, stirred and emulsified to obtain a silicone waterborne polyurethane adhesive.

[0026] Example 2

[0027] (1) Add 30 parts by weight of 1,1,3,3-tetramethyl-1,3-bis[3-(oxiranylmethoxy)propyl]disiloxane and 600 mL of N,N-dimethylformamide to a reaction flask, mix well, add 48 parts of sodium p-aminobenzenesulfonate, react at 70° C. for 8 h, concentrate, and recrystallize the product in an ethanol aqueous solution with a volume fraction of 80% to obtain a sodium bishydroxysiloxane benzenesulfonate monomer.

[0028] (2) In a four-necked flask equipped with a thermometer, a condenser reflux tube and a stirrer, 100 parts of polytetramethylene glycol, 35 parts of isophorone diisocyanate and 1.5 parts of dibutyltin dilaurate as a catalyst were added by weight, stirred at 80°C for 2 hours, and then 35 parts of sodium bishydroxysiloxane benzenesulfonate monomer were added and reacted for 1 hour. Then, 2.3 parts of KH550 were added for end-capping, the reaction system was cooled to 30°C, and deionized water was slowly added to the system, stirred and emulsified to obtain a silicone waterborne polyurethane adhesive.

[0029] Example 3

[0030] (1) Add 5 parts by weight of 1,1,3,3-tetramethyl-1,3-bis[3-(oxiranylmethoxy)propyl]disiloxane and 50 mL of N,N-dimethylformamide to a reaction flask, mix well, add 5.8 parts of sodium p-aminobenzenesulfonate, react at 55° C. for 16 h, concentrate, and recrystallize the product in a 70% by volume ethanol aqueous solution to obtain a sodium bishydroxysiloxane benzenesulfonate monomer.

[0031] (2) In a four-necked flask equipped with a thermometer, a condenser reflux tube and a stirrer, 100 parts of polytetramethylene glycol, 28 parts of isophorone diisocyanate and 0.8 parts of dibutyltin dilaurate as a catalyst were added by weight, and stirred at 70°C for 3 hours. Then, 38 parts of sodium bishydroxysiloxane benzenesulfonate monomer were added and reacted for 1.5 hours. Then, 3.6 parts of KH550 were added for end-capping. The reaction system was cooled to 30°C, and deionized water was slowly added to the system. The mixture was stirred and emulsified to obtain a silicone waterborne polyurethane adhesive.

[0032] Example 4

[0033] (1) Add 15 parts by weight of 1,1,3,3-tetramethyl-1,3-bis[3-(oxiranylmethoxy)propyl]disiloxane and 240 mL of N,N-dimethylformamide to a reaction flask, mix well, add 21 parts of sodium p-aminobenzenesulfonate, react at 60° C. for 15 h, concentrate, and recrystallize the product in an ethanol aqueous solution with a volume fraction of 80% to obtain a sodium bishydroxysiloxane benzenesulfonate monomer.

[0034] (2) In a four-necked flask equipped with a thermometer, a condenser reflux tube and a stirrer, 100 parts of polytetramethylene glycol, 33 parts of isophorone diisocyanate and 1.1 parts of dibutyltin dilaurate as a catalyst were added by weight, and stirred at 75°C for 3 hours. Then, 40 parts of sodium bishydroxysiloxane benzenesulfonate monomer were added and reacted for 1 hour. Then, 5 parts of KH550 were added for end-capping. The reaction system was cooled to 30°C, and deionized water was slowly added to the system. The mixture was stirred and emulsified to obtain a silicone waterborne polyurethane adhesive.

[0035] Comparative Example 1

[0036] In a four-necked flask equipped with a thermometer, a condenser reflux tube and a stirrer, 100 parts of polytetramethylene ether diol, 30 parts of isophorone diisocyanate and 1.2 parts of dibutyltin dilaurate as a catalyst were added by weight, and stirred at 75°C for 3 hours. Then, 1 part of KH550 was added for end-capping. The reaction system was cooled to 30°C, and deionized water was slowly added to the system, stirred and emulsified to obtain a water-based polyurethane adhesive.

[0037] Water resistance test: Pour the silicone water-based polyurethane adhesive into a glass tank, place it horizontally in a 60°C oven for 24 hours to form a film, and after the water evaporates slowly, place it in a 70°C vacuum oven to dry for 48 hours, then place it in the air for a week. After the adhesive is completely cured, make a film sample, weigh a certain mass (m1) of the film sample, soak it in distilled water for 12 hours, then take it out, use filter paper to absorb the surface moisture and weigh it as m2, water absorption (%) = (m1-m2) / m1.

[0038] Table 1 Emulsion stability and water absorption test results of Examples 1-4 and Comparative Example 1

[0039]

[0040] It can be seen from the test results in the above table that with the introduction of sodium bishydroxysiloxane benzene sulfonate monomer and KH550, the emulsion stability in the polyurethane system is good, and there is no precipitation after being placed for 7 days. The sodium sulfonate in its structure has strong hydrophilicity, which makes the polyurethane dispersion have a more stable "double electric layer" structure, and has better compatibility with the silicone waterborne polyurethane adhesive system, and the dispersion performance is better; at the same time, the water absorption rate of the film decreases with the increase of silicone content, reaching a minimum of 0.51%. This is because the sodium bishydroxysiloxane benzene sulfonate monomer contains Si-O-Si structure and has a lower surface tension, which reduces the surface energy of the system. In the film-forming stage of the polyurethane adhesive, the hydrophobic silicone segment migrates to the surface of the material, and the remaining segments migrate to the inside of the material, so that the water resistance of the adhesive has been improved to a certain extent, so the prepared silicone waterborne polyurethane adhesive has better comprehensive performance. Comparative Example 1 does not contain sodium bishydroxysiloxane benzene sulfonate monomer, and its emulsion dispersibility is poor and the water resistance is poor.

[0041] Example 5

[0042] Add 45 parts of kaolin, 20 parts of quartz, 8 parts of high white sodium feldspar, 6 parts of wollastonite, 9 parts of potassium feldspar, 10 parts of spodumene and 2 parts of silicon nitride whiskers by weight into a ball mill, mill the mixture, pass through a 220-mesh sieve, add 20 parts of deionized water to granulate, and after pressing into shape with an electric hydraulic brick machine, transfer to a silicon carbon rod furnace, heat at a heating rate of 6°C / min, sinter at 1000°C for 4 hours, and naturally cool to obtain a crack-resistant ceramic rock plate.

[0043] Example 6

[0044] 46 parts of kaolin, 15 parts of quartz, 10 parts of high white sodium feldspar, 4 parts of wollastonite, 3 parts of potassium feldspar, 13 parts of spodumene and 4 parts of silicon nitride whiskers by weight are added into a ball mill, the mixture is ball-milled and passed through a 200-mesh sieve, 30 parts of deionized water are added for granulation, and the mixture is pressed into shape by an electric hydraulic brick machine, and then transferred to a silicon carbon rod furnace, heated at a heating rate of 8°C / min, sintered at 1000°C for 5 hours, and naturally cooled to obtain a crack-resistant ceramic rock plate.

[0045] Example 7

[0046] Add 24 parts of kaolin, 25 parts of quartz, 10 parts of high white sodium feldspar, 8 parts of wollastonite, 12 parts of potassium feldspar, 15 parts of spodumene and 6 parts of silicon nitride whiskers by weight into a ball mill, mill the mixture, pass through a 300-mesh sieve, add 25 parts of deionized water to granulate, and after pressing into shape with an electric hydraulic brick machine, transfer to a silicon carbon rod furnace, heat at a heating rate of 7°C / min, sinter at 1050°C for 5 hours, and naturally cool to obtain a crack-resistant ceramic rock plate.

[0047] Example 8

[0048] Add 36 parts of kaolin, 22 parts of quartz, 6 parts of high white sodium feldspar, 7 parts of wollastonite, 9 parts of potassium feldspar, 12 parts of spodumene and 8 parts of silicon nitride whiskers by weight into a ball mill, mill the mixture, pass through a 260-mesh sieve, add 20 parts of deionized water to granulate, and after pressing into shape with an electric hydraulic brick machine, transfer to a silicon carbon rod furnace, heat at a heating rate of 5°C / min, sinter at 1200°C for 4 hours, and naturally cool to obtain a crack-resistant ceramic rock plate.

[0049] Example 9

[0050] Add 20 parts of kaolin, 25 parts of quartz, 10 parts of high white sodium feldspar, 8 parts of wollastonite, 12 parts of potassium feldspar, 15 parts of spodumene and 10 parts of silicon nitride whiskers by weight into a ball mill, mill the mixture, pass through a 240-mesh sieve, add 25 parts of deionized water to granulate, and after pressing and molding with an electric hydraulic brick machine, transfer to a silicon carbon rod furnace, heat at a heating rate of 6°C / min, sinter at 1150°C for 5 hours, and naturally cool to obtain a crack-resistant ceramic rock plate.

[0051] Comparative Example 2

[0052] Add 45 parts of kaolin, 20 parts of quartz, 8 parts of high white sodium feldspar, 6 parts of wollastonite, 9 parts of potassium feldspar and 10 parts of spodumene in weight into a ball mill, mill the mixture, pass through a 220-mesh sieve, add 20 parts of deionized water to granulate, and after pressing into shape with an electric hydraulic brick machine, transfer to a silicon carbon rod furnace, heat at a heating rate of 6°C / min, sinter at 1000°C for 4 hours, and naturally cool to obtain a ceramic rock plate.

[0053] Rupture modulus test: The rupture modulus of ceramic rock slabs is determined according to GB / T 3810.4-2016 "Test methods for ceramic tiles Part 4: Determination of rupture modulus and breaking strength".

[0054] Table 2 Determination results of the modulus of rupture of ceramic rock panels

[0055] Modulus of rupture (MPa) Example 5 64.8 Example 6 83.6 Example 7 89.5 Example 8 95.0 Example 9 93.7 Comparative Example 2 50.3

[0056] Generally speaking, the higher the modulus of rupture, the better the toughness and strength of the material, and the greater the destructive force it can withstand. From the test results in the above table, it can be seen that with the increase of the content of silicon nitride whiskers in the ceramic rock plate, the modulus of rupture of the ceramic rock plate gradually increases. This is because silicon nitride whiskers have good physical and chemical compatibility with the ceramic phase. After the introduction of silicon nitride whiskers into the ceramic body, a reinforcing phase is effectively formed, so that the interface between the two is better. Therefore, under the action of external loads, the whiskers can be partially digested and dispersed to a certain extent, and at the same time, the crack expansion path is effectively extended, so that the sample fracture requires more energy, and the fracture strength of the ceramic rock plate is enhanced, which has better crack resistance. In Comparative Example 2, silicon nitride whiskers were not added, and the modulus of rupture of the ceramic rock plate was only 50.3MPa, which was easily damaged by external loads.

[0057] Example 10

[0058] Before construction, check and clean the base layer. The height error is about 3mm. The silicone water-based polyurethane adhesive (prepared by Example 3) is evenly applied to the upper surface of the base layer with the serrated edge of a V-shaped plastering knife with a tooth depth of 3mm. The thickness of the adhesive layer is 1mm. After the adhesive and the base layer are fully infiltrated, the surface of the anti-cracking ceramic rock board (prepared by Example 8) is polished with sandpaper. After cleaning and drying, the adhesive is applied to the lower surface of the anti-cracking ceramic rock board with the straight edge of the plastering knife. Then, the applied anti-cracking ceramic rock board is pasted to the upper surface of the base layer coated with the silicone water-based polyurethane adhesive, and the vibrator is used for leveling and compacting.

[0059] Embodiment 11

[0060] Before construction, check and clean the base layer. The height error is about 2mm. The silicone water-based polyurethane adhesive (prepared by Example 3) is evenly applied to the upper surface of the base layer with the serrated edge of a U-shaped plastering knife with a tooth depth of 1mm. The thickness of the adhesive layer is 3mm. After the adhesive and the base layer are fully infiltrated, the surface of the anti-cracking ceramic rock board (prepared by Example 8) is polished with sandpaper. After cleaning and drying, the adhesive is applied to the lower surface of the anti-cracking ceramic rock board with the straight edge of the plastering knife. Then, the applied anti-cracking ceramic rock board is pasted to the upper surface of the base layer coated with the silicone water-based polyurethane adhesive, and the vibrator is used for leveling and compacting.

[0061] Example 12

[0062] Before construction, check and clean the base layer. The height error is about 0.1mm. The silicone water-based polyurethane adhesive (prepared by Example 3) is evenly applied to the upper surface of the base layer with the serrated edge of a V-shaped plastering knife with a tooth depth of 8mm. The thickness of the adhesive layer is 5mm. After the adhesive and the base layer are fully infiltrated, the surface of the anti-cracking ceramic rock board (prepared by Example 8) is polished with sandpaper. After cleaning and drying, the adhesive is applied to the lower surface of the anti-cracking ceramic rock board with the straight edge of the plastering knife. Then, the applied anti-cracking ceramic rock board is pasted to the upper surface of the base layer coated with the silicone water-based polyurethane adhesive, and the vibrator is used for leveling and compacting.

[0063] Comparative Example 3

[0064] Before construction, check and clean the base layer. The height error is about 3mm. Use the serrated edge of a V-shaped plastering knife with a tooth depth of 1mm to evenly apply ordinary tile adhesive on the upper surface of the base layer. The thickness of the adhesive layer is 5mm. After the ordinary tile adhesive and the base layer are fully infiltrated, use sandpaper to polish the surface of the anti-cracking ceramic rock board (prepared by Example 8). After cleaning and drying, use the straight edge of the plastering knife to flatten the lower surface of the anti-cracking ceramic rock board with ordinary tile adhesive and apply a layer. Then, paste the applied anti-cracking ceramic rock board on the upper surface of the base layer coated with ordinary tile adhesive, and use a vibrator to level and compact.

[0065] According to the relevant provisions of "Ceramic Wall and Floor Tile Adhesive" (JC / T547-2017), the tensile bond strength tests under normal conditions, hot and cold shocks and freeze-thaw cycles were carried out. The preparation, maintenance and performance test methods of the specimens were carried out in accordance with the provisions.

[0066] Table 3 Test results of bonding layer thickness and tensile bond strength of Examples 10-12 and Comparative Example 3

[0067]

[0068] It can be seen from the test results in the above table that the thickness of the bonding layer of Example 10 is only 1 mm, and the tensile bonding strength of the ceramic rock slab under normal conditions is 1.39 MPa. Even after freeze-thaw cycles and hot and cold shocks, the tensile strength does not change much, and it has strong bonding performance; while the bonding layer of Comparative Example 3 uses ordinary tile adhesive, which has a thicker bonding layer thickness and lower tensile bonding strength. It debonds after hot and cold shocks, and has poor bonding performance; it can be seen that the paving process of the present invention can achieve ultra-thin paving, and the thickness of the bonding layer can be reduced by up to 80%, which simplifies the paving process of ceramic rock slabs and does not use cement sand for paving, achieving the goal of lightweight and low labor intensity; this paving process is in line with the environmental protection concept of energy saving and emission reduction in terms of bonding layer thickness, material density, construction efficiency, transportation cost, materials, production and energy consumption during construction, and greatly reduces carbon emissions.

[0069] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A paving process for crack-resistant ceramic rock slabs, characterized in that: The invention comprises the following components in parts by weight: 20-46 parts of kaolin, 15-25 parts of quartz, 5-10 parts of high-white sodium feldspar, 4-8 parts of wollastonite, 3-12 parts of potassium feldspar, 5-15 parts of spodumene, and 2-10 parts of silicon nitride whiskers; the preparation method of the anti-cracking ceramic rock plate comprises the following steps: adding kaolin, quartz, high-white sodium feldspar, potassium feldspar, spodumene, wollastonite, and silicon nitride whiskers into a ball mill, ball milling the mixture, passing through a 200-300 mesh sieve, adding 10-30 parts of deionized water for granulation, pressing and forming the mixture with an electric hydraulic brick machine, transferring the mixture to a silicon carbon rod furnace, sintering the mixture, and naturally cooling the mixture to obtain the anti-cracking ceramic rock plate; The sintering temperature is 1000-1200°C, the sintering time is 3-5h, and the heating rate is 5-8°C / min; The paving process comprises the following steps: Before construction, check and clean the base layer. The height error should be between 0.1-3mm. Use the serrated edge of the plastering knife to evenly apply the silicone water-based polyurethane adhesive to the upper surface of the base layer to form a glue layer. After the adhesive and the base layer are fully infiltrated, use sandpaper to polish the surface of the anti-cracking ceramic rock plate. After cleaning and drying, use the straight edge of the plastering knife to flatten the adhesive on the lower surface of the anti-cracking ceramic rock plate and apply a layer. Then, stick the applied anti-cracking ceramic rock plate to the upper surface of the base layer coated with the silicone water-based polyurethane adhesive. Use a vibrator to level and compact. The preparation method of the organic silicone waterborne polyurethane adhesive comprises the following steps: (1) adding 1,1,3,3-tetramethyl-1,3-bis[3-(oxiranylmethoxy)propyl]disiloxane and N,N-dimethylformamide to a reaction flask, mixing them evenly, adding sodium p-aminobenzenesulfonate, stirring for reaction, concentrating after the reaction is completed, and recrystallizing the product in an ethanol aqueous solution to obtain a sodium bishydroxysiloxane benzenesulfonate monomer; (2) Add polytetrahydrofuran ether diol, isophorone diisocyanate and catalyst dibutyltin dilaurate to a four-necked flask equipped with a thermometer, a condenser reflux tube and a stirrer, stir at 70-80° C. for 2-3 hours, then add sodium bishydroxysiloxane benzenesulfonate monomer, react for 1-1.5 hours, then add KH550 for end-capping, cool the reaction system to 30° C., add deionized water to the system, stir and emulsify, and obtain a silicone waterborne polyurethane adhesive; In the step (1), the amount of 1,1,3,3-tetramethyl-1,3-bis[3-(oxiranylmethoxy)propyl]disiloxane is 100 parts by weight and the amount of sodium p-aminobenzenesulfonate is 115-160 parts by weight; In the step (2), by weight, the polytetramethylene glycol is 100 parts, the isophorone diisocyanate is 28-35 parts, the dibutyltin dilaurate is 0.8-1.5 parts, the sodium bishydroxysiloxane benzenesulfonate monomer is 32-40 parts, and the KH550 is 1-5 parts.

2. The paving process of the anti-crack ceramic rock slab according to claim 1 is characterized in that: The thickness of the adhesive layer is 1-5 mm.

3. The paving process of the anti-crack ceramic rock slab according to claim 1 is characterized in that: The plastering tooth knife is a V-shaped plastering tooth knife or a U-shaped plastering tooth knife, and the tooth depth is 1-8mm.

4. The paving process of the anti-crack ceramic rock slab according to claim 1 is characterized in that: In the preparation method of the organic silicone waterborne polyurethane adhesive, the reaction temperature in step (1) is 55-70° C. and the reaction time is 8-16 hours.