Polarizing sheet, polarizing lens, and optical component
The polarizing sheet with polyurethane adhesive bonding layers maintains transparency and adhesion in polarized lenses by controlling haze and adhesion strength, addressing issues in existing thermal bending and molding processes.
Patent Information
- Application Number
- JP2023059444
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing polarized lenses experience a decrease in transparency due to thermal bending and injection molding processes, especially when exposed to high temperatures, leading to issues with haze and adhesion strength.
A polarizing sheet composed of a uniaxially stretched polarizing film sandwiched between protective sheets with polyurethane adhesive bonding layers, designed to maintain a haze value of 0.05% to 1.00% even after exposure to high temperatures, ensuring reliable adhesion and transparency.
The solution effectively prevents transparency loss and maintains adhesion strength in polarized lenses, even under high-temperature conditions, resulting in highly reliable optical components.
Smart Images

Figure 2024146499000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polarizing sheet, a polarizing lens, and an optical component. [Background technology]
[0002] A polarizing lens has been proposed that includes a polarizing laminate (polarizing sheet) in which both sides of a polarizing film are covered with coating layers made primarily of polycarbonate-based resin or polyamide-based resin (see, for example, Patent Document 1).
[0003] This polarizing lens is manufactured, for example, by punching a polarizing laminate (polarizing sheet) having a flat plate shape in plan view into a predetermined shape such as a circle in plan view with protective films attached to both sides of the polarizing laminate. Then, the polarizing laminate is subjected to a heat bending process under heating to form a polarizing sheet having a curved plate shape by heat bending. Then, after peeling off the protective film from the polarizing sheet, the polarizing sheet is adsorbed on a mold having a curved plate-shaped recess so that the recess of the mold and the protrusion of the polarizing sheet come into contact with each other, and a resin layer (optical lens) mainly made of a resin material such as a polycarbonate resin or a polyamide resin is formed on the concave surface of the polarizing sheet by injection molding.
[0004] Furthermore, a hard coat layer is formed as the outermost layer on at least one surface of the polarizing lens depending on its application.
[0005] In the polarizing laminate provided in such a polarizing lens, the polarizing film and the covering layer are bonded via a bonding layer, and a polyurethane-based adhesive may be used for this bonding layer in consideration of its transparency and bonding strength.
[0006] However, in this case, when a polarizing lens is manufactured by applying the above-mentioned manufacturing method for a polarizing lens, there is a problem in that the transparency of the polarizing laminate is reduced after the heat bending process of the polarizing laminate (polarizing sheet) under heating, after the injection molding of the resin layer (optical lens), and further after the formation of the hard coat layer.
[0007] Furthermore, this problem, i.e., a decrease in transparency in the polarizing laminate, also occurs when sunglasses (eyeglasses) equipped with the polarizing lenses are placed for a long period of time in a high-temperature space, such as the dashboard of a car. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2009-294445 A Summary of the Invention [Problem to be solved by the invention]
[0009] An object of the present invention is to provide a polarizing sheet in which loss of transparency is appropriately suppressed or prevented even when exposed to high temperatures, and to provide a highly reliable polarizing lens and optical component that are equipped with such a polarizing sheet. [Means for solving the problem]
[0010] Such an object can be achieved by the present invention described in the following (1) to (11). (1) A polarizing sheet comprising: a polarizing film that is uniaxially stretched and has an absorption axis in the direction of the uniaxial stretching; a first protective sheet having birefringence laminated on one surface of the polarizing film; a second protective sheet having the same or higher birefringence as the first protective sheet laminated on the other surface of the polarizing film; a first bonding layer bonding the polarizing film and the first protective sheet; and a second bonding layer bonding the polarizing film and the second protective sheet, The first bonding layer and the second bonding layer are each formed mainly of a polyurethane adhesive; A polarizing sheet characterized in that, when the haze value of the polarizing sheet is measured in accordance with JIS K 7136:2000 after immersing the polarizing sheet in distilled water at 80°C for 15 minutes, the haze value is 0.05% or more and 1.00% or less.
[0011] (2) The polarizing sheet according to (1) above, in which when the polarizing sheet is immersed in distilled water at 80°C for 15 minutes in accordance with JIS K 7136:2000 and the adhesion strength of the polarizing sheet is measured, the adhesion strength satisfies the following requirement A and the following requirement B. Requirement A: In accordance with JIS K 6854-2, the polarizing sheet is cut to a size of 200 mm in length × 25 mm in width, and then, in an environment of 140°C, one end of the first protective sheet of the polarizing sheet is held and peeled off to a length of 10 mm in a direction of 180° at a speed of 10 mm / min to a length of 10 mm. The adhesion strength of the first protective sheet to the polarizing film, as measured, satisfies a requirement of 40 N / 25 mm or more and 500 N / 25 mm or less. Requirement B: In accordance with JIS K 6854-2, the polarizing sheet is cut to a size of 200 mm in length × 25 mm in width, and then, in an environment of 140°C, one end of the second protective sheet of the polarizing sheet is held and peeled off to a length of 10 mm in a direction of 180° at a speed of 10 mm / min. The adhesion strength of the second protective sheet to the polarizing film, measured when the second protective sheet is peeled off to a length of 10 mm, satisfies the requirement of 40 N / 25 mm or more and 500 N / 25 mm or less.
[0012] (3) The polarizing sheet according to (1) or (2) above, wherein the polyurethane adhesive is a one-component moisture crosslinking type or a two-component crosslinking type.
[0013] (4) The polarizing sheet according to any one of (1) to (3) above, wherein the first protective sheet and the second protective sheet are each made primarily of a polycarbonate-based resin or a polyamide-based resin.
[0014] (5) The polarizing sheet according to any one of (1) to (4) above, wherein the polarizing film is made of a polyvinyl alcohol resin or a derivative thereof as a main material, contains a dichroic dye, and is uniaxially stretched.
[0015] (6) The polarizing sheet according to any one of (1) to (5) above, wherein the polarizing sheet is curved so that the first protective sheet forms a concave surface and the second protective sheet forms a convex surface, the polarizing sheet is placed in a cavity of a mold of an injection molding machine so that the convex side of the polarizing sheet faces the mold of the injection molding machine and the concave side is exposed, and is used to form an optical lens to be bonded to the first protective sheet by injection molding, the optical lens being made mainly of an optical resin for injection molding.
[0016] (7) A polarizing lens comprising: the polarizing sheet according to any one of (1) to (6) above, in which the first protective sheet forms a concave surface and the second protective sheet forms a convex surface to form a curved plate; and the optical lens bonded to the first protective sheet on the concave surface and formed by injection molding.
[0017] (8) The polarized lens according to (7) above, wherein when the haze value of the polarized lens is measured in accordance with JIS K 7136:2000 after immersing the polarized lens in distilled water at 80°C for 15 minutes, the haze value is 0.05% or more and 1.00% or less.
[0018] (9) The polarized lens according to (7) or (8) above, wherein, when the polarized lens is used, the concave surface of the polarizing sheet facing the first protective sheet faces the user's eyes.
[0019] (10) The polarized lens according to any one of (7) to (9) above, wherein in the polarizing sheet included in the polarized lens, the difference between the curve in MD and the curve in TD is 0.05 or more and 0.5 or less.
[0020] (11) An optical component comprising the polarizing lens according to any one of (7) to (10) above. Effect of the Invention
[0021] According to the present invention, when the haze value of the polarizing sheet is measured after immersing the polarizing sheet in distilled water at 80°C for 15 minutes in accordance with JIS 7136:2000, the haze value is 0.05% or more and 1.00% or less. Therefore, even if the polarizing sheet is exposed to high temperatures, such as when the polarizing sheet is subjected to heat bending processing under heating or injection molding of an optical lens to manufacture a polarizing lens equipped with the polarizing sheet, it can be said that the decrease in transparency of the polarizing sheet is appropriately suppressed or prevented. Therefore, it is possible to manufacture polarizing lenses and optical components with excellent reliability. [Brief description of the drawings]
[0022] [Figure 1] FIG. 11 is a perspective view showing an embodiment in which the present invention is applied to sunglasses as an optical component equipped with a polarizing lens having a polarizing sheet. [Diagram 2] 1A to 1C are schematic diagrams illustrating a method for producing a polarizing lens having a polarizing sheet of the present invention. [Diagram 3] 1 is a vertical cross-sectional view showing an embodiment of a polarizing sheet of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The polarizing sheet, polarizing lens, and optical component of the present invention will be described in detail below with reference to preferred embodiments shown in the accompanying drawings. In this specification, the term "main material" refers to a constituent material that is contained at 50% by weight or more. For example, "the first protective sheet contains a polycarbonate-based resin as its main material" means that, when the total weight of the first protective sheet is taken as 100% by weight, the polycarbonate-based resin contained in the first protective sheet accounts for 50% by weight or more of the first protective sheet.
[0024] The polarizing sheet 10 of the present invention includes a polarizing film 13, a first protective sheet 11 laminated on one side of the polarizing film 13, a second protective sheet 12 laminated on the other side of the polarizing film, a first bonding layer 16 bonding the polarizing film 13 to the first protective sheet 11, and a second bonding layer 17 bonding the polarizing film 13 to the second protective sheet 12. The polarizing sheet 10 is curved such that the first protective sheet 11 forms a concave surface and the second protective sheet 12 forms a convex surface, and the polarizing sheet 10 is placed in a cavity of a mold 40 of an injection molding machine such that the convex surface side of the polarizing sheet 10 faces the mold 40 of the injection molding machine and the concave surface side is exposed. The polarizing sheet 10 is used to form, by injection molding, a resin layer 35 (optical lens) to be bonded to the first protective sheet 11, the resin layer 35 being made mainly of an optical resin for injection molding. The first bonding layer 16 and the second bonding layer 17 are each made mainly of a polyurethane-based adhesive and are formed in accordance with JIS Z 11011-1999. In accordance with 7136:2000, when the haze value of polarizing sheet 10 is measured after immersing polarizing sheet 10 in distilled water at 80° C. for 15 minutes, the haze value satisfies a requirement of 0.05% or more and 1.00% or less.
[0025] Therefore, even if the polarizing sheet 10 is exposed to high temperatures, such as when the polarizing sheet 10 is subjected to heat bending processing under heating or injection molding of the resin layer 35 (optical lens) during the manufacture of the polarizing lens 30 including the polarizing sheet 10, it can be said that a decrease in the transparency of the polarizing sheet 10 is appropriately suppressed or prevented. Thus, a highly reliable polarizing lens 30 and sunglasses 100 as an optical component can be manufactured.
[0026] The polarizing sheet 10 of the present invention is used, for example, as a polarizing resin substrate of a polarizing lens 30 provided in sunglasses 100, which is a type of eyeglasses serving as an optical component. Therefore, in the following, first, the sunglasses 100 (the optical component of the present invention) will be described before describing the polarizing sheet 10 of the present invention.
[0027] <Sunglasses> Fig. 1 is a perspective view showing an embodiment in which the optical component having a polarizing lens having the polarizing sheet of the present invention is applied to sunglasses. In Fig. 1, when the sunglasses are worn on the head of a user, the surface of the lens facing the user's eyes is called the back surface, and the opposite surface is called the front surface.
[0028] As shown in FIG. 1, sunglasses 100 include a frame 20 and a polarized lens 30 (the polarized lens of the present invention).
[0029] In this specification, the term "polarized lens" includes both lenses that have a light-collecting function and lenses that do not have a light-collecting function.
[0030] The frame 20 is fitted to the head of a user so that the polarized lenses 30 are positioned in front of and near the user's eyes.
[0031] The frame 20 has a rim portion 21, a bridge portion 22, a temple portion 23, and a nose pad portion 24.
[0032] The rim portion 21 is ring-shaped, and one is provided for each of the right and left eyes, and a polarized lens 30 is attached to the inside. This allows the user to view external information through the polarized lens 30.
[0033] Furthermore, the bridge portion 22 is rod-shaped and is positioned in front of the upper part of the user's nose when the glasses are worn on the user's head, connecting the pair of rim portions 21 together.
[0034] The temple portion 23 is shaped like a temple and is connected to the edge of each rim portion 21 on the opposite side to the position where the bridge portion 22 is connected. The temple portion 23 is hung on the user's ear when wearing the glasses on the user's head.
[0035] The nose pads 24 are provided on the edges of the rims 21 that correspond to the nose of the user when the sunglasses 100 are worn on the head of the user, and come into contact with the nose of the user, forming a shape that corresponds to the contact portion of the nose of the user at this time. This allows the sunglasses 100 to be stably maintained when worn.
[0036] The materials constituting the respective parts of the frame 20 are not particularly limited, and may be, for example, various metal materials, various resin materials, etc. The shape of the frame 20 is not limited to that shown in the figure, so long as it can be worn on the head of the user.
[0037] A polarizing lens 30 is attached to each rim portion 21. This polarizing lens 30 is a light-transmitting, plate-shaped member curved toward the outside, i.e., a member with a curved convex surface facing the outside and a concave surface facing the user's eyes.
[0038] The resin layer 35 is optically transparent and is located on the back side of the polarized lens 30 to function as an optical lens. When the polarized lens 30 is given a light-collecting function, this resin layer 35 has the light-collecting function.
[0039] The constituent material used as the main material of resin layer 35 (optical lens) is not particularly limited as long as it is a resin material (optical resin for injection molding) that has optical transparency and can be used to form resin layer 35 by injection molding, as explained in the manufacturing method of polarized lens 30 described below. Examples of the material include various thermoplastic resins, thermosetting resins, and various curable resins such as photocurable resins, and one or a combination of two or more of these can be used.
[0040] Examples of the resin material (optical resin for injection molding) include polyolefins such as polyethylene, polypropylene, and ethylene-propylene copolymers, polyvinyl chloride, polystyrene, polyamide, polyimide, polycarbonate, poly-(4-methylpentene-1), ionomers, acrylic resins, polymethyl methacrylate, acrylonitrile-butadiene-styrene copolymers (ABS resins), acrylonitrile-styrene copolymers (AS resins), butadiene-styrene copolymers, polyesters such as polyethylene terephthalate (PET) and polybutylene terephthalate (PBT), polyethers, polyether ketones (PEK), poly Examples of the resin include ether ether ketone (PEEK), polyetherimide, polyacetal (POM), polyphenylene oxide, polysulfone, polyethersulfone, polyphenylene sulfide, polyarylate, aromatic polyester (liquid crystal polymer), polytetrafluoroethylene, polyvinylidene fluoride, other fluorine-based resins, epoxy resins, phenolic resins, urea resins, melamine resins, silicone resins, polyurethanes, etc., or copolymers, blends, polymer alloys, etc., mainly made of these resins. Among these, it is preferable that the resin layer 35 is the same as or identical to the resin material constituting the first protective sheet 11 of the polarizing sheet 10 described below. This allows excellent adhesion to be exhibited between the resin layer 35 and the polarizing sheet 10, and therefore it is possible to appropriately suppress or prevent the resin layer 35 from being separated from the polarizing sheet 10.
[0041] The thickness of resin layer 35 is not particularly limited, and is, for example, preferably 0.5 mm to 5.0 mm, and more preferably 1.0 mm to 3.0 mm, which allows polarized lens 30 to have both relatively high strength and light weight.
[0042] The polarizing sheet 10 is a polarizing resin substrate that is bonded to the outer surface of the resin layer 35, i.e., the curved convex surface, after being subjected to a heat bending process into a curved plate shape corresponding to the shape, thereby imparting polarization to the sunglasses 100. As a result, the sunglasses 100 exhibit the function of polarized sunglasses having polarization. This polarizing sheet 10 is composed of the polarizing sheet of the present invention, but a detailed explanation of it will be given later.
[0043] As described above, the polarized lenses 30 of the sunglasses 100 may or may not have a light-collecting function.
[0044] Furthermore, as described above, the sunglasses 100 may have the frame 20, or may have a frameless configuration from the standpoint of fashionability, lightweightness, and the like.
[0045] Furthermore, in this embodiment, the optical component of the present invention is applied to sunglasses 100, but is not limited to this, and the optical component of the present invention may be, for example, prescription glasses, glasses such as fashion glasses, goggles that protect the eyes from wind, rain, dust, chemicals, etc., face shields, visors, and goggles for smart glasses.
[0046] In sunglasses 100 configured as described above, polarized lens 30 (polarized lens of the present invention) provided in sunglasses 100 is manufactured by the manufacturing method of polarized lens 30 described below in the present invention.
[0047] <Polarizing lens manufacturing method> 2 is a schematic diagram for explaining the method for producing a polarizing lens having a polarizing sheet of the present invention. For convenience of explanation, the upper side of FIG. 1 will be referred to as "top" and the lower side as "bottom."
[0048] Each step of the method for producing a polarizing lens 30 equipped with a polarizing sheet 10 of the present invention will be described in detail below.
[0049] [1] First, a polarizing sheet 10 is prepared, which includes a first protective sheet 11, a polarizing film 13, and a second protective sheet 12, which are laminated in this order to have an overall flat shape. Then, protective films 50 (masking tape) are attached to both sides of the polarizing sheet 10, thereby obtaining a multilayer laminate 200 in which the protective films 50 are attached to both sides of the polarizing sheet 10 (see FIG. 1(a)).
[0050] [2] Next, as shown in FIG. 1(b), the prepared multilayer laminate 200, i.e., the polarizing sheet 10 with protective films 50 attached to both sides thereof, is punched out in its thickness direction, so that the multilayer laminate 200 has a circular shape in a plan view.
[0051] [3] Next, as shown in FIG. 1(c), the circular multilayer laminate 200 is subjected to a heat bending process under heating.
[0052] This gives the multilayer laminate 200 a curved plate shape with the first protective sheet 11 side being a curved concave surface (concave surface) and the second protective sheet 12 side being a curved convex surface (convex surface). As a result, with the protective films 50 attached to both sides, the polarizing sheet 10 has a curved plate shape with the first protective sheet 11 side being a curved concave surface (concave surface) and the second protective sheet 12 side being a curved convex surface (convex surface).
[0053] Furthermore, by subjecting the multilayer laminate 200 to a heat bending process, the polarizing sheet 10 has a difference between the curve in MD and the curve in TD set to preferably 0.05 to 0.5, more preferably 0.05 to 0.2.
[0054] This heat bending is usually carried out by press forming or vacuum forming. As described above, in this embodiment, the heating temperature (molding temperature) of the multilayer laminate 200 (polarizing sheet 10) is set to about 110° C. or more and 170° C. or less, more preferably about 140° C. or more and 160° C. or less, taking into consideration the melting or softening temperatures of the protective sheets 11, 12, in which the polarizing sheet 10 includes the protective sheets 11, 12. By setting the heating temperature within this range, the polarizing sheet 10 can be brought into a softened or molten state while preventing alteration or deterioration of the polarizing sheet 10, and the polarizing sheet 10 can be reliably thermally bent to form, for example, a curved plate-like polarizing sheet 10 in which the difference between the curve in MD and the curve in TD is set within the above range.
[0055] It is preferable to perform a drying step of drying the multilayer laminate 200 prior to the heat bending process in step [3]. This can adequately suppress or prevent deformation of the polarizing sheet 10 due to moisture absorption, and therefore the heat bending process of the multilayer laminate 200, i.e., the heat bending process of the polarizing sheet 10 with the protective films 50 attached to both sides, can be performed with excellent accuracy. The drying of the multilayer laminate 200 can be performed, for example, by blowing hot air of about 70° C. to 80° C. onto the surface of the multilayer laminate 200 for a time period of about 5 hours to 15 hours.
[0056] [4] Next, the protective film 50 is peeled off from the thermally bent polarizing sheet 10, i.e., the multilayer laminate 200. Thereafter, as shown in FIG. 2(d), the polarizing sheet 10 is placed in a state of being adsorbed to a mold 40 of an injection molding machine having a curved concave surface shaped like a curved plate, with the curved concave surface of the mold 40 and the curved convex surface of the polarizing sheet 10, i.e., the second protective sheet 12 side, being in contact with each other. As a result, the polarizing sheet 10 is placed in the cavity 401 of the mold 40 with the curved concave surface of the polarizing sheet 10, i.e., the first protective sheet 11 side, exposed. Then, in this state, a resin layer 35 made of a resin material is injection molded on the curved concave surface (first protective sheet 11) of the polarizing sheet 10 using an insert injection molding method (injection molding method). As a result, a polarizing lens 30 is manufactured that includes the thermally bent polarizing sheet 10 and the resin layer 35 (optical lens).
[0057] Among the insert injection molding methods, the injection compression molding method is preferably used. The injection compression molding method is a method in which a resin material (optical resin for injection molding) for forming the resin layer 35 is injected into the mold 40 at low pressure, and then the mold 40 is closed at high pressure to apply a compressive force to the resin material, so that the resin layer 35 as a molded body, and in turn the polarized lens 30, are less likely to suffer from molding distortion or optical anisotropy due to the local orientation of the resin molecules during molding, and is therefore preferably used. In addition, by controlling the mold compression force that is uniformly applied to the resin material, the resin material can be cooled at a constant specific volume, so that the resin layer 35 with high dimensional accuracy can be obtained.
[0058] It is preferable to perform a drying step of drying the heat-bent polarizing sheet 10 prior to forming the resin layer 35 in step [4]. This makes it possible to appropriately suppress or prevent deformation of the heat-bent polarizing sheet 10 due to moisture absorption, and therefore allows the resin layer 35 to be molded with excellent accuracy on the heat-bent polarizing sheet 10. As a result, the polarized lens 30 including the polarizing sheet 10 and the resin layer 35 can be obtained with higher dimensional accuracy. The drying of the polarizing sheet 10 can be performed, for example, by blowing hot air of about 75°C to 85°C onto the surface of the polarizing sheet 10 for a time period of about 15 minutes to 2 hours.
[0059] Furthermore, this polarized lens 30 may be provided with a hard coat layer as an outermost layer on at least one side thereof depending on the application. This hard coat layer can be formed, for example, by applying a thermosetting resin composition to the surface of polarized lens 30, followed by heating and drying. In this case, the resin composition can be heated and dried, for example, by blowing hot air at a temperature of about 100° C. or higher and 130° C. or lower onto the surface of polarizing sheet 10 for a period of about 1 hour to 3 hours.
[0060] The polarizing sheet of the present invention is used as the polarizing sheet 10 used in the manufacturing method of the polarizing lens 30 described above, and therefore, when the haze value of the polarizing sheet 10 is measured after immersing the polarizing sheet 10 in distilled water at 80° C. for 15 minutes in accordance with JIS K 7136:2000, the haze value satisfies 0.05% or more and 1.00% or less. Therefore, even if the polarizing sheet 10 is subjected to heat bending processing under heating or injection molding of the resin layer 35 (optical lens) during the manufacture of the polarizing lens 30 including the polarizing sheet 10, it can be said that a decrease in the transparency of the polarizing sheet 10 is appropriately suppressed or prevented, and the polarizing sheet of the present invention will be described in detail below.
[0061] <Polarizing sheet 10> Polarizing sheet 10 (polarizing sheet of the present invention) is a polarizing laminate including a polarizing film 13, a first protective sheet 11 laminated on one side of polarizing film 13, a second protective sheet 12 laminated on the other side of polarizing film 13, a first bonding layer 16 bonding polarizing film 13 to first protective sheet 11, and a second bonding layer 17 bonding polarizing film 13 to second protective sheet 12. Each component (each layer) constituting polarizing sheet 10 will be described below.
[0062] 3 is a vertical cross-sectional view showing an embodiment of the polarizing sheet of the present invention. For convenience of explanation, the upper side of FIG. 1 will be referred to as "upper" and the lower side as "lower".
[0063] (Polarizing Film 13) The polarizing film 13 is uniaxially stretched and has an absorption axis in the direction of this uniaxial stretching, and thus has the function of extracting linearly polarized light having a polarization plane in the direction of the uniaxial stretching from incident light (unpolarized natural light). As a result, the light passing through the polarizing sheet 10 becomes polarized.
[0064] The polarization degree of the polarizing film 13 is not particularly limited, but is preferably, for example, from 50% to 100%, and more preferably from 80% to 100%. The visible light transmittance of the polarizing film 13 is not particularly limited, but is preferably, for example, from 10% to 80%, and more preferably from 20% to 50%.
[0065] The material constituting such polarizing film 13 is not particularly limited as long as it has the above-mentioned functions, and examples thereof include polyvinyl alcohol (PVA), partially formalized polyvinyl alcohol, polyethylene vinyl alcohol, polyvinyl butyral, polycarbonate, and partially saponified ethylene-vinyl acetate copolymer. Examples of polarizing film 13 include a polymer film made of any of these constituent materials, which is dyed with a dichroic substance such as iodine or a dichroic dye and then uniaxially stretched.
[0066] Among these, the polarizing film 13 is preferably a polymer film mainly made of polyvinyl alcohol (PVA), which is dyed with iodine or a dichroic dye and uniaxially stretched. Polyvinyl alcohol (PVA) is a material that is excellent in transparency, heat resistance, affinity with the dyeing agent iodine or a dichroic dye, and orientation during stretching. Therefore, the polarizing film 13 mainly made of PVA has excellent heat resistance and polarizing ability.
[0067] Examples of the dichroic dye include Chloratin Fast Red, Congo Red, Brilliant Blue 6B, Benzopurpurine, Chlorazol Black BH, Direct Blue 2B, Diamine Green, Chrysophenone, Sirius Yellow, Direct Fast Red, and Acid Black.
[0068] The thickness of the polarizing film 13 is not particularly limited, and is preferably, for example, from 5 μm to 60 μm, and more preferably from 10 μm to 40 μm.
[0069] (First protective sheet 11) The first protective sheet 11 is a resin layer having birefringence, and as shown in Figures 2(d) and 3, is laminated on the lower surface (one of the surfaces) of the polarizing film 13, i.e., the curved concave surface (concave surface), and thereby functions as a protective layer that protects the lower surface of the polarizing film 13.
[0070] This first protective sheet 11 is not particularly limited as long as it has birefringence, but for example, it is mainly made of resin materials such as polyamide-based resin and polycarbonate-based resin, and one or more of these resin materials can be used in combination. By making the first protective sheet 11 mainly made of at least one of polyamide-based resin and polycarbonate-based resin, it is possible to make the first protective sheet 11 have a relatively high birefringence.
[0071] Polycarbonate-based resins are excellent in transparency (light transmissivity) and mechanical strength such as rigidity, and therefore can improve the transparency and impact resistance of the polarizing sheet 10. Furthermore, polycarbonate-based resins have a specific gravity of about 1.2, and are classified as light among resin materials, which can reduce the weight of the polarizing sheet 10. Furthermore, polyamide-based resins can improve the chemical resistance, stress resistance, and the like, in addition to the transparency and impact resistance.
[0072] The polyamide resin is not particularly limited, and various types can be used, such as alicyclic polyamide and semi-aromatic polyamide. Alicyclic polyamide is a material with excellent impact resistance. Therefore, the polarizing sheet 10 can be made to exhibit excellent impact resistance. Semi-aromatic polyamide is a material with a high elastic modulus. Therefore, the polarizing sheet 10 can be made to have excellent resistance to stress such as bending.
[0073] In this specification, semi-aromatic polyamide refers to a polyamide in which one of the dicarboxylic acid and diamine monomers constituting the polyamide is an aromatic compound and the other is an aliphatic compound, and specifically, can be represented by the following formula (1B).
[0074] [ka] (However, R in formula (1B) 1 and R 2 one of which is a divalent aromatic substituent and the other is a divalent aliphatic substituent, and n is an integer of 2 or greater.
[0075] The polyamide may be a copolymer (random copolymer, block copolymer, etc.) containing two or more kinds of monomers of at least one of dicarboxylic acid and diamine.
[0076] In addition, R in the above formula (1B) 1 , R 2 Of these, the aromatic substituent is preferably one represented by the following formula (2B).
[0077] [ka] (In formula (2B), l and m each independently represent an integer of 0 or more and 2 or less.)
[0078] This can provide better protection for the polarizing film 13 and improve the processability of the polarizing sheet 10. Furthermore, when retardation is imparted to the first protective sheet 11, it is possible to more easily control the retardation by stretching the first protective sheet 11. The same effect can be obtained even when the second protective sheet 12 contains this polyamide resin.
[0079] R in the above formula (1B) 1 , R 2 Of these, the aliphatic substituent is preferably one having 4 to 18 carbon atoms, more preferably a hydrocarbon group having 4 to 18 carbon atoms, and even more preferably a saturated hydrocarbon group having 4 to 18 carbon atoms. This can improve the processability of the polarizing sheet 10.
[0080] Furthermore, the semi-aromatic polyamide preferably contains an aromatic dicarboxylic acid and an aliphatic diamine as constituent monomers. This can better protect the polarizing film 13 and improve the processability of the polarizing sheet 10. In addition, retardation control by stretching can be more easily performed.
[0081] An alicyclic polyamide has an alicyclic chemical structure in its molecule, and may have an alicyclic chemical structure in its main chain structure or may have an alicyclic chemical structure in its side chain structure.
[0082] Examples of the alicyclic polyamide include compounds in which at least one of the dicarboxylic acid and diamine monomers constituting the polyamide has an alicyclic chemical structure, and specifically, for example, can be represented by the following formula (3B).
[0083] [ka] (In formula (3B), R 3 , R 4 are each independently a hydrogen atom or a hydrocarbon group having 4 or less carbon atoms, o is an integer of 2 or more and 14 or less, p is an integer of 0 or more and 6 or less, and n is an integer of 2 or more.
[0084] The polycarbonate resin is not particularly limited and various types can be used, but among them, aromatic polycarbonate resins are preferable. Aromatic polycarbonate resins have aromatic rings in their main chains, which can improve the strength of the polarizing sheet 10.
[0085] The aromatic polycarbonate resin is synthesized, for example, by an interfacial polycondensation reaction between bisphenol and phosgene, or an ester exchange reaction between bisphenol and diphenyl carbonate.
[0086] Examples of bisphenols include bisphenol A and bisphenol (modified bisphenol) which is the source of the repeating unit of polycarbonate represented by the following formula (1A).
[0087] [ka] (In formula (1A), X is an alkyl group having 1 to 18 carbon atoms, an aromatic group, or a cyclic aliphatic group; Ra and Rb are each independently an alkyl group having 1 to 12 carbon atoms; m and n are each an integer of 0 to 4; and p is the number of repeating units.)
[0088] Specific examples of bisphenols that are the source of the repeating units of the polycarbonate represented by the formula (1A) include 4,4'-(pentane-2,2-diyl)diphenol, 4,4'-(pentane-3,3-diyl)diphenol, 4,4'-(butane-2,2-diyl)diphenol, 1,1'-(cyclohexanediyl)diphenol, 2-cyclohexyl-1,4-bis(4-hydroxyphenyl)benzene, 2,3-biscyclohexyl-1,4-bis(4-hydroxyphenyl)benzene, 1,1'-bis(4-hydroxy-3-methylphenyl)cyclohexane, and 2,2'-bis(4-hydroxy-3-methylphenyl)propane, and any of these may be used alone or in combination of two or more.
[0089] In particular, the polycarbonate resin may contain a bisphenol-type polycarbonate resin having a skeleton derived from bisphenol, and is preferably composed mainly of a bisphenol-type polycarbonate resin having a skeleton derived from bisphenol. By using such a bisphenol-type polycarbonate resin, the polarizing sheet 10 exhibits even greater strength.
[0090] The glass transition temperature (Tg) of the resin material contained as the main material in the first protective sheet 11 is preferably 100°C or higher and 190°C or lower, and more preferably 105°C or higher and 155°C or lower. This allows the heat bending process of the polarizing sheet 10 in the step [3] to be carried out relatively easily. Furthermore, when the first protective sheet 11 and the second protective sheet 12 are caused to exhibit retardation such that the retardation of the second protective sheet 12 is higher, stretching for the exhibiting of this retardation can be suitably carried out. Furthermore, the durability and reliability of the polarizing sheet 10 can be improved.
[0091] Furthermore, in addition to the resin material contained as the main material, first protective sheet 11 may contain other components. Such components are not particularly limited, but may include, for example, a resin material other than the main material, a colorant such as a dye, a filler, an alignment aid, a stabilizer (such as a heat stabilizer, an ultraviolet absorber, and an antioxidant), a plasticizer, a colorant, a flame retardant, an antistatic agent, and a viscosity adjuster.
[0092] In this case, the content of the resin material in first protective sheet 11 is not particularly limited, but is preferably 75 parts by mass or more, and more preferably 85 parts by mass or more, per 100 parts by mass of first protective sheet 11. By setting the content of the resin material within the above range, polarizing sheet 10 can exhibit excellent strength.
[0093] The retardation of the first protective sheet 11 is preferably lower than that of the second protective sheet 12, and specifically, for example, is preferably 0 nm or more and 5000 nm or less, and more preferably 50 nm or more and 350 nm or less. This allows the polarization performance of the polarizing sheet 10 to be fully exhibited. In addition, by setting the retardation of the first protective sheet 11 within the above range, and further setting the retardation of the second protective sheet 12 within a range described below, the polarizing sheet 10 can achieve both a particularly high level of processability and durability.
[0094] The difference in retardation of first protective sheet 11 can be realized by varying the constituent materials contained in the layer, the thickness, and further the stretching ratio.
[0095] There are no particular limitations on the average thickness of first protective sheet 11, and it is preferably, for example, from 0.05 mm to 0.5 mm, and more preferably from 0.1 mm to 0.4 mm.
[0096] The stretching ratio of first protective sheet 11 is not particularly limited, but is preferably, for example, from 0.95 to 1.1 so as to be set in accordance with the magnitude of the retardation.
[0097] It is also preferable that the stretching directions of the first protective sheet 11 and the polarizing film 13 are the same, which can further improve the polarizing performance of the polarizing sheet 10.
[0098] (Second protective sheet 12) The second protective sheet 12 is a resin layer having the same or higher birefringence as that of the first protective sheet 11, and is laminated on the upper surface (the other surface) of the polarizing film 13, i.e., the curved convex surface (convex surface), as shown in Figures 2(d) and 3, and thereby functions as a protective layer that protects the upper surface side of the polarizing film 13.
[0099] Like the first protective sheet 11, the second protective sheet 12 is primarily made of resin materials such as polyamide-based resin and polycarbonate-based resin, and is set to have the same or a higher birefringence than the first protective sheet 11 by using one or a combination of two or more of these resin materials.
[0100] As the polyamide-based resin and polycarbonate-based resin, the same materials as those listed above as the constituent materials of first protective sheet 11 can be used.
[0101] The glass transition temperature (Tg) of the resin material contained as the main material in the second protective sheet 12 is preferably 100°C or higher and 190°C or lower, and more preferably 105°C or higher and 155°C or lower, similar to that of the first protective sheet 11. This allows the heat bending process of the polarizing sheet 10 in the step [3] to be carried out relatively easily. Furthermore, when the first protective sheet 11 and the second protective sheet 12 are caused to exhibit retardation, with the second protective sheet 12 exhibiting a higher retardation, stretching for the exhibiting of this retardation can be suitably carried out. Furthermore, the durability and reliability of the polarizing sheet 10 can be improved.
[0102] Furthermore, in addition to the resin material contained as the main material, second protective sheet 12 may contain other components. Such components are not particularly limited, but include, for example, resin materials other than the main material, colorants such as dyes, fillers, alignment aids, stabilizers (heat stabilizers, ultraviolet absorbers, antioxidants, etc.), plasticizers, colorants, flame retardants, antistatic agents, viscosity adjusters, etc.
[0103] In this case, the content of the resin material in second protective sheet 12 is not particularly limited, but is preferably 75 parts by mass or more, and more preferably 85 parts by mass or more, per 100 parts by mass of second protective sheet 12. By setting the content of the resin material within the above range, polarizing sheet 10 can exhibit excellent strength.
[0104] The retardation of the second protective sheet 12 is preferably higher than that of the first protective sheet 11, and specifically, for example, is preferably 2600 nm or more and 8000 nm or less, and more preferably 3500 nm or more and 6500 nm or less. This allows the polarizing performance of the polarizing sheet 10 to be fully exhibited. In addition, when the polarizing sheet 10 is subjected to the heat bending process in the step [3], the effect of preventing rainbow color unevenness and color fading can be obtained.
[0105] The difference in retardation of the second protective sheet 12 can be realized by varying the constituent materials contained in the layer, the thickness, and further the stretching ratio.
[0106] The average thickness of second protective sheet 12 is not particularly limited, and is, for example, preferably 0.05 mm or more and 0.5 mm or less, and more preferably 0.1 mm or more and 0.4 mm or less.
[0107] The stretching ratio of second protective sheet 12 is not particularly limited, but is preferably set to the magnitude of the retardation, for example, from 1.5 to 3.5.
[0108] It is also preferable that the stretching directions of the second protective sheet 12 and the polarizing film 13 are the same, which can further improve the polarizing performance of the polarizing sheet 10.
[0109] (First bonding layer 16, second bonding layer 17) The first bonding layer 16 (first adhesive layer) has the function of bonding the polarizing film 13 and the first protective sheet 11, and the second bonding layer 17 (second adhesive layer) has the function of bonding the polarizing film 13 and the second protective sheet 12, thereby improving the durability of the polarizing sheet 10.
[0110] In the present invention, a polyurethane adhesive is used as the adhesive (or pressure-sensitive adhesive) constituting the first bonding layer 16 and the second bonding layer 17. This can make the first bonding layer 16 and the second bonding layer 17 particularly excellent in terms of conformability to changes in shape while providing the first bonding layer 16 and the second bonding layer 17 with more excellent transparency, adhesive strength, and durability. For this reason, in the present invention, a polyurethane adhesive is used as the adhesive constituting the first bonding layer 16 and the second bonding layer 17.
[0111] Here, the polyurethane adhesive contains a polyisocyanate compound having an isocyanate group as a constituent material in order to function as an adhesive. When this isocyanate group reacts with water in the air, etc., it generates carbon dioxide via carbamic acid and forms an amino group.
[0112] Furthermore, as described above, when first protective sheet 11 and second protective sheet 12 are primarily made of a resin material such as a polyamide-based resin or a polycarbonate-based resin, first protective sheet 11 and second protective sheet 12 exhibit excellent gas barrier properties. In particular, such gas barrier properties are more significantly exhibited when first protective sheet 11 and second protective sheet 12 are primarily made of a polyamide-based resin.
[0113] In this way, when the first protective sheet 11 and the second protective sheet 12 exhibit excellent gas barrier properties, the carbon dioxide generated in the first bonding layer 16 and the second bonding layer 17 remains in the first bonding layer 16 and the second bonding layer 17, which causes bubbles to be generated in the first bonding layer 16 and the second bonding layer 17. The generation of bubbles causes a problem of reducing the transparency of the first protective sheet 11 and the second protective sheet 12. In particular, the generation of bubbles is frequently observed when the polarizing sheet is exposed to high temperatures, for example, when performing heat bending or injection molding accompanied by heat treatment in the manufacturing method of the polarizing lens described above. The present inventor's investigation has revealed that this is due to the fact that isocyanate groups derived from isocyanate compounds remain in the first bonding layer 16 and the second bonding layer 17, and that the carbon dioxide generated by the reaction of the remaining isocyanate groups with water in the air or the like during the heat treatment is caused by this.
[0114] In contrast, in the present invention, when the haze value of the polarizing sheet 10 is measured after immersing the polarizing sheet 10 in distilled water at 80° C. for 15 minutes in accordance with JIS K 7136:2000, the haze value satisfies 0.05% or more and 1.00% or less. In this way, in the present invention, the haze value satisfies 0.05% or more and 1.00% or less, and it can be said that the decrease in transparency of the first protective sheet 11 and the second protective sheet 12 due to exposure to high temperatures such as the heat treatment is appropriately suppressed, and the generation of bubbles in the first bonding layer 16 and the second bonding layer 17 provided in the polarizing sheet 10 is appropriately suppressed or prevented.
[0115] In addition, the suppression of the generation of air bubbles in the first bonding layer 16 and the second bonding layer 17 can be achieved, for example, as follows, depending on the type of polyurethane-based adhesive contained in the first bonding layer 16 and the second bonding layer 17, i.e., whether the polyurethane-based adhesive is a two-component crosslinking type or a one-component moisture crosslinking type.
[0116] That is, when the polyurethane adhesive is a two-part crosslinking type containing a polyisocyanate compound and a polyol, the polyisocyanate compound reacts with the polyol to form a urethane bond between them, and the adhesive hardens. In this two-part crosslinking polyurethane adhesive, the polyisocyanate compound is usually contained in the adhesive at a functional group equivalent of about 1.2 times the polyol, assuming that the polyisocyanate compound reacts with moisture in the air and is deactivated. However, if the polyurethane adhesive contains a large amount of polyisocyanate compound with such a functional group equivalent relative to the polyol, the bonding layer formed with this polyurethane adhesive naturally tends to have unreacted isocyanate groups remaining. Therefore, when a polarizing sheet having such a bonding layer is exposed to high temperatures, such as when a heat bending process or injection molding is performed with a heat treatment, bubbles are generated in the bonding layer due to the generation of carbon dioxide. In contrast, in the present invention, a polyisocyanate compound is contained in the adhesive at a functional group equivalent of about 1.0 times, i.e., the same functional group equivalent, relative to the polyol, to suppress the remaining of unreacted isocyanate groups in the first bonding layer 16 and the second bonding layer 17. Therefore, even if the polarizing sheet 10 is exposed to high temperatures, such as when performing hot bending or injection molding involving heat treatment, the generation of bubbles in the first bonding layer 16 and the second bonding layer 17 is appropriately suppressed. Therefore, the haze value can be set within a range of 0.05% to 1.00%.
[0117] In addition, when the polyurethane adhesive is a one-component moisture crosslinking type that does not contain polyol and contains diisocyanates at both ends as polyisocyanate compounds, the diisocyanates at both ends react with water in the air or the like to generate carbon dioxide and an amino group-containing compound having an amino group. Then, the other diisocyanates at both ends react with this amino group-containing compound to form a urea bond between them, and the adhesive hardens. In this way, in a one-component moisture crosslinking type polyurethane adhesive, carbon dioxide is usually generated by reacting the diisocyanates at both ends with water. Therefore, when a polarizing sheet having a bonding layer derived from such a one-component moisture crosslinking type polyurethane adhesive is exposed to a high temperature, such as when a heat bending process or injection molding is performed with a heat treatment, the diisocyanates at both ends remaining in the bonding layer react with water, and bubbles are generated in the bonding layer due to the generation of carbon dioxide. In contrast, in the present invention, the first bonding layer 16 and the second bonding layer 17 are configured to further contain a trifunctional isocyanate in addition to the diisocyanates at both ends. As a result, in the first bonding layer 16 and the second bonding layer 17, a compound in which a six-membered ring is formed by the reaction of three isocyanate groups is generated, and the reaction between the diisocyanate at both ends and water is inhibited. Therefore, even if the polarizing sheet 10 is exposed to high temperatures, such as when performing hot bending processing or injection molding involving heat treatment, the generation of bubbles in the first bonding layer 16 and the second bonding layer 17 is appropriately suppressed. Therefore, the haze value can be set within a range of 0.05% to 1.00%.
[0118] Here, between a two-component crosslinking polyurethane adhesive and a one-component moisture crosslinking polyurethane adhesive, the two-component crosslinking polyurethane adhesive is superior to the one-component moisture crosslinking polyurethane adhesive in terms of the effect of suppressing the generation of bubbles in the first bonding layer 16 and the second bonding layer 17. Therefore, when the first protective sheet 11 and the second protective sheet 12 are composed mainly of a polyamide resin, a two-component crosslinking polyurethane adhesive is particularly preferably selected as the polyurethane adhesive contained in the first bonding layer 16 and the second bonding layer 17.
[0119] In addition, when the haze value of the polarizing sheet 10 is measured after immersing the polarizing sheet 10 in distilled water at 80° C. for 15 minutes in accordance with JIS K 7136:2000, the haze value may be 0.05% or more and 1.00% or less, but the haze value is preferably 0.05% or more and 0.50% or less, and more preferably 0.05% or more and 0.20% or less. This can be said to more accurately suppress or prevent the generation of bubbles in the first bonding layer 16 and the second bonding layer 17 of the polarizing sheet 10.
[0120] Furthermore, in a polarizing lens 30 equipped with a polarizing sheet 10 that satisfies such a haze value, when the haze value of the polarizing lens 30 is measured after immersing the polarizing lens 30 in distilled water at 80° C. for 15 minutes in accordance with JIS K 7136:2000, the haze value is preferably 0.05% or more and 1.00% or less, and more preferably 0.05% or more and 0.50% or less. This means that the generation of bubbles in the first bonding layer 16 and second bonding layer 17 of the polarizing sheet 10 of the polarizing lens 30 is more appropriately suppressed or prevented.
[0121] Furthermore, when the adhesion strength of the polarizing sheet 10 is measured in accordance with JIS K 7136:2000 after immersing the polarizing sheet in distilled water at 80°C for 15 minutes, it is preferable that the adhesion strength satisfies the following requirement A and the following requirement B.
[0122] That is, polarizing sheet 10 is cut to a size of 200 mm in length × 25 mm in width in accordance with JIS K 6854-2, and then one end of first protective sheet 11 of polarizing sheet 10 is held and peeled off to a length of 10 mm at a speed of 10 mm / min in a 180° direction in an environment of 140° C. The adhesion strength of first protective sheet 11 to polarizing film 13 measured when the sheet is cut in accordance with JIS K 6854-2 is preferably 40 N / 25 mm or more and 500 N / 25 mm or less, more preferably 50 N / 25 mm or more and 300 N / 25 mm or less, and even more preferably 80 N / 25 mm or more and 250 N / 25 mm or less (requirement A).
[0123] Furthermore, polarizing sheet 10 is cut to a size of 200 mm in length × 25 mm in width in accordance with JIS K 6854-2, and then one end of second protective sheet 12 of polarizing sheet 10 is held and peeled off to a length of 10 mm at a speed of 10 mm / min in a direction of 180° in a 140° C. environment. The adhesion strength of second protective sheet 12 to polarizing film 13 is measured as follows: it is preferably 40 N / 25 mm or more and 500 N / 25 mm or less, more preferably 50 N / 25 mm or more and 300 N / 25 mm or less, and even more preferably 80 N / 25 mm or more and 250 N / 25 mm or less (requirement B).
[0124] When air bubbles are generated in the polarizing sheet 10, as described above, the transparency of the polarizing sheet 10 tends to decrease, and in addition, the adhesive strength of the first bonding layer 16 and the second protective sheet 12 tends to decrease. In contrast, in the present invention, the polarizing sheet 10 can be made to satisfy the requirements A and B relatively easily, and therefore, when the polarizing sheet 10 is subjected to a heat bending process or injection molding involving a heat treatment, the occurrence of cracks in the polarizing sheet 10 can be appropriately suppressed or prevented, while the adhesive strength of the first bonding layer 16 and the second protective sheet 12 can be appropriately suppressed or prevented from decreasing. Therefore, it can be said that the occurrence of air bubbles in the first bonding layer 16 and the second protective sheet 12 is appropriately suppressed.
[0125] The thickness of first bonding layer 16 and second bonding layer 17 is not particularly limited, and is preferably, for example, 5 μm to 60 μm, more preferably 10 μm to 40 μm, so that the function of first bonding layer 16 can be reliably imparted.
[0126] In addition to the case where heat bending processing or injection molding involving heating is performed, even when a hard coat layer is formed on the polarizing sheet 10 so that the polarizing lens 30 has a hard coat layer as its outermost layer, or even when it is assumed that the sunglasses 100 will be placed for a long period of time in a high-temperature space such as the dashboard of a car, in the present invention, as described above, the generation of air bubbles in the first bonding layer 16 of the polarizing sheet 10 is appropriately suppressed, and the haze value can be set within the range of 0.05% or more and 1.00% or less.
[0127] Although the polarizing sheet, polarizing lens, and optical component of the present invention have been described above, the present invention is not limited to these.
[0128] For example, each part constituting the polarizing sheet of the present invention can be replaced with any other part having a similar function.
[0129] Furthermore, the polarizing sheet of the present invention may further include any other component in addition to the above-mentioned components.
[0130] More specifically, for example, the polarizing sheet of the present invention may include an intermediate layer, a power adjusting layer for adjusting the power of the lens, and the like. EXAMPLES
[0131] The present invention will be described in detail below based on examples, but the present invention is not limited thereto.
[0132] 1. Manufacturing of polarizing sheets Example 1A First, a polyvinyl alcohol-based film was dyed with an aqueous solution containing a dye while being stretched in a water tank, and then treated with boric acid. The treated polyvinyl alcohol-based film was then washed with water and dried. This resulted in a polarizing film 13 having a thickness of 35 μm.
[0133] Meanwhile, a polycarbonate resin (manufactured by Mitsubishi Gas Chemical Co., Ltd., "Iupilon E-2000") was extrusion molded using a vented single screw extruder to obtain a sheet-like first protective sheet 11 with a thickness of 0.2 mm and a retardation of 4200 nm.
[0134] Also, a polycarbonate resin (manufactured by Mitsubishi Gas Chemical Co., Ltd., "Iupilon E-2000") was extrusion molded using a vented single-screw extruder to obtain a sheet-like second protective sheet 12 with a thickness of 0.2 mm and a retardation of 4200 nm.
[0135] Next, on one side of the first protective sheet 11, a two-component moisture-curing polyurethane adhesive (main agent (polyol): Mitsui Chemicals, Inc., "Takelac A-520", curing agent (polyisocyanate compound): Mitsui Chemicals, Inc., "Takenate A-50", functional group equivalent; main agent: curing agent = 1.0: 1.0) was applied as a first adhesive with a bar coater so that the thickness of the first bonding layer 16 after drying was 20 μm. Also, on one side of the second protective sheet 12, a two-component moisture-curing polyurethane adhesive (main agent (polyol): Mitsui Chemicals, Inc., "Takelac A-520", curing agent (polyisocyanate compound): Mitsui Chemicals, Inc., "Takenate A-50", functional group equivalent; main agent: curing agent = 1.0: 1.0) was applied as a second adhesive with a bar coater so that the thickness of the second bonding layer 17 after drying was 20 μm.
[0136] Next, the first protective sheet 11 and the second protective sheet 12, on which the first adhesive and the second adhesive were respectively applied, were placed in an oven and heated until the solvent in the first adhesive and the second adhesive was dried. This resulted in a first laminate in which a first bonding layer 16 (first adhesive layer) was laminated on one surface of the first protective sheet 11, and a second laminate in which a second bonding layer 17 (second adhesive layer) was laminated on one surface of the second protective sheet 12.
[0137] Thereafter, the first laminate was laminated on the polarizing film 13 so that the first adhesive layer 16 was in contact with one surface of the polarizing film 13, and the second laminate was laminated on the polarizing film 13 so that the second adhesive layer 17 was in contact with the other surface of the polarizing film 13, thereby obtaining a polarizing sheet 10 of Example 1A. At this time, the first laminate, the polarizing film 13, and the second laminate were each pressed together using a rubber roll of a laminator machine, and the total thickness of the polarizing sheet 10 was set to 0.75 mm. After obtaining the polarizing sheet 10, the first adhesive and the second adhesive contained in the first adhesive layer 16 and the second adhesive layer 17, respectively, were completely cured by curing for one week in a 30°C environment.
[0138] (Examples 2A to 6A, Comparative Examples 1A to 3A) The polarizing sheets 10 of Examples 2A to 6A and Comparative Examples 1A to 3A were obtained in the same manner as in Example 1A, except that the polyurethane-based adhesive used to form the first bonding layer 16 and the second bonding layer 17 of the polarizing sheet 10 had a functional group equivalence relationship as shown in Table 1.
[0139] The one-component moisture crosslinking polyurethane adhesive used was one having diisocyanates at both ends (manufactured by Mitsui Chemicals, Inc., "LA2355") and trifunctional isocyanate (manufactured by DIC Corporation, "DN-902S").
[0140] Example 1B Polarizing sheet 10 of Example 1B was obtained in the same manner as in Example 1A, except that sheet-like first protective sheet 11 and second protective sheet 12 were each obtained as follows.
[0141] That is, first protective sheet 11 was made of a polyamide resin ("Grilamid TR90" manufactured by EMS) and was obtained by extrusion molding using a vented single-screw extruder in the form of a sheet with a thickness of 0.4 mm and a retardation of 0 nm.
[0142] Second protective sheet 12 was made of a polyamide resin ("Grilamid TR90" manufactured by EMS) and was obtained by extrusion molding using a vented single-screw extruder in the form of a sheet with a thickness of 0.2 mm and a retardation of 2600 nm.
[0143] (Examples 2B to 3B, Reference Examples 1B to 3B, Comparative Examples 1B to 3B) The polarizing sheets 10 of Examples 2B to 3B, Reference Examples 1B to 3B, and Comparative Examples 1B to 3B were obtained in the same manner as in Example 1B, except that the polyurethane-based adhesive used to form the first bonding layer 16 and the second bonding layer 17 of the polarizing sheet 10 had a functional group equivalence relationship as shown in Table 2.
[0144] The one-component moisture crosslinking polyurethane adhesive used was one having diisocyanates at both ends (manufactured by Mitsui Chemicals, Inc., "LA2355") and trifunctional isocyanate (manufactured by DIC Corporation, "DN-902S").
[0145] 2. Evaluation The polarizing sheets of each of the Examples and Comparative Examples were evaluated by the following method.
[0146] <1> Measuring the haze value of polarizing sheets First, the polarizing sheets of each of the examples and comparative examples were immersed in distilled water at 80° C. for 15 minutes in accordance with JIS K 7136:2000. Thereafter, the haze value of the polarizing sheets was measured using a haze meter (manufactured by Nippon Denshoku Kogyo Co., Ltd., “NDH4000”).
[0147] <2-1> Measurement of adhesion of the first protective sheet to the polarizing sheet First, the polarizing sheets of each of the examples and comparative examples were immersed in distilled water at 80° C. for 15 minutes in accordance with JIS K 7136:2000. Thereafter, in accordance with JIS K 6854-2, the polarizing sheets were cut to a size of 200 mm in length and 25 mm in width, and then, in an environment of 140° C., one end of the first protective sheet of the polarizing sheet was held and peeled off to a length of 10 mm at a speed of 10 mm / min in a direction of 180°, and the adhesion strength of the first protective sheet to the polarizing film was measured using a tensile tester (manufactured by Shimadzu Corporation, “AG-10kNXplus”) (requirement A).
[0148] <2-2> Measurement of adhesion of the first protective sheet to the polarizing sheet First, the polarizing sheets of each of the examples and comparative examples were immersed in distilled water at 80° C. for 15 minutes in accordance with JIS K 7136:2000. Thereafter, in accordance with JIS K 6854-2, the polarizing sheets were cut to a size of 200 mm in length and 25 mm in width, and then, in an environment of 140° C., one end of the second protective sheet of the polarizing sheet was held and peeled off to a length of 10 mm at a speed of 10 mm / min in a direction of 180°, and the adhesion strength of the second protective sheet to the polarizing film was measured using a tensile tester (manufactured by Shimadzu Corporation, “AG-10kNXplus”) (requirement B).
[0149] <3> Measuring the haze value of polarized lenses First, for each of the polarizing sheets in each of the Examples and Comparative Examples, a protective film made of polyolefin was laminated by a lamination method on both sides of the polarizing sheet, i.e., on the side of the first protective sheet opposite the polarizing film, and on the side of the second protective sheet opposite the polarizing film.
[0150] Next, this polarizing sheet was punched out to a diameter of 8 cm, and then subjected to hot bending processing while applying suction at 150°C for 10 minutes using a Rema molding machine (vacuum molding machine) (CR-32 type), to produce a polarizing sheet with a radius of curvature R1 in MD of 80.5 mm and a radius of curvature R2 in TD of 87.2 mm.
[0151] Next, the protective film was peeled off from the heat-bent polarizing sheet 10, and then a resin layer composed of an optical resin for injection molding (manufactured by Mitsubishi Gas Chemical Co., Ltd., "H-3000") was formed by injection molding on the curved concave surface (first protective sheet) side of the polarizing sheet 10 using a mold 40 shown in Figure 2(d), thereby obtaining a polarizing lens.
[0152] Then, in accordance with JIS K 7136:2000, each of the obtained polarized lenses was immersed in distilled water at 80° C. for 15 minutes. Thereafter, the haze value of this polarized lens was measured using a haze meter (manufactured by Nippon Denshoku Kogyo Co., Ltd., "NDH4000").
[0153] <4> Evaluating the presence of air bubbles in polarized lenses First, for each of the polarizing sheets in each of the Examples and Comparative Examples, a protective film made of polyolefin was laminated by a lamination method on both sides of the polarizing sheet, i.e., on the side of the first protective sheet opposite the polarizing film, and on the side of the second protective sheet opposite the polarizing film.
[0154] Next, this polarizing sheet was punched out to a diameter of 8 cm, and then subjected to hot bending processing while applying suction at 150°C for 10 minutes using a Rema molding machine (vacuum molding machine) (CR-32 type), to produce a polarizing sheet with a radius of curvature R1 in MD of 80.5 mm and a radius of curvature R2 in TD of 87.2 mm.
[0155] Next, the protective film was peeled off from the heat-bent polarizing sheet 10, and then a resin layer composed of an optical resin for injection molding (manufactured by Mitsubishi Gas Chemical Co., Ltd., "H-3000") was formed by injection molding on the curved concave surface (first protective sheet) side of the polarizing sheet 10 using a mold 40 shown in Figure 2(d), thereby obtaining a polarizing lens.
[0156] The resulting polarized lenses were then visually inspected for the presence or absence of air bubbles, and were rated as follows: ⊚ when no air bubbles were found, ◯ when a few air bubbles were found, △ when air bubbles were definitely found, and × when air bubbles were clearly found.
[0157] The evaluation results of the polarizing sheets of the respective Examples and Comparative Examples thus obtained are shown in the following Tables 1 and 2, respectively.
[0158] [Table 1]
[0159] [Table 2]
[0160] As shown in Tables 1 and 2, in each example, the haze value in the polarizing sheet was greater than or equal to 0.05% and less than or equal to 1.00%, thereby demonstrating that when a polarizing lens is obtained, the generation of air bubbles in the polarizing sheet provided in the polarizing lens can be appropriately suppressed or prevented.
[0161] In contrast, in each of the comparative examples, the haze value in the polarizing sheet did not satisfy the requirement of 0.05% or more and 1.00% or less, and as a result, the generation of air bubbles was observed in the polarizing sheet provided with the polarizing lens when the polarizing lens was obtained. [Explanation of symbols]
[0162] 10 Polarizing Sheet 11 First protective sheet 12 Second protective sheet 13 Polarizing film 16 1st bonding layer 17 Second bonding layer 20 Frames 21 Rim 22 Bridge section 23 Temple Section 24 Nose pad section 30 Polarized Lenses 35 Resin layer 40 Mold 50 Protective Film 100 Sunglasses 200 Multilayer laminate 401 Cavity
Claims
1. A polarizing sheet comprising: a polarizing film that is uniaxially stretched and has an absorption axis in the direction of the uniaxial stretching; a first protective sheet having birefringence laminated on one surface of the polarizing film; a second protective sheet having the same or higher birefringence as the first protective sheet laminated on the other surface of the polarizing film; a first bonding layer bonding the polarizing film and the first protective sheet; and a second bonding layer bonding the polarizing film and the second protective sheet, The first bonding layer and the second bonding layer are each formed mainly of a polyurethane adhesive, A polarizing sheet characterized in that, when the haze value of the polarizing sheet is measured after immersing the polarizing sheet in distilled water at 80°C for 15 minutes in accordance with JIS K 7136:2000, the haze value is 0.05% or more and 1.00% or less.
2. The polarizing sheet according to claim 1, wherein when the adhesion of the polarizing sheet is measured after immersing the polarizing sheet in distilled water at 80°C for 15 minutes in accordance with JIS K 7136:2000, the adhesion satisfies the following requirement A and the following requirement B. Requirement A: In accordance with JIS K 6854-2, the polarizing sheet is cut to a size of 200 mm in length × 25 mm in width, and then, in an environment of 140° C., one end of the first protective sheet of the polarizing sheet is held and peeled off to a length of 10 mm at a speed of 10 mm / min in a direction of 180°, and the adhesion strength of the first protective sheet to the polarizing film, measured when the first protective sheet is peeled off to a length of 10 mm, satisfies the requirement of 40 N / 25 mm or more and 500 N / 25 mm or less. Requirement B: In accordance with JIS K 6854-2, the polarizing sheet is cut to a size of 200 mm in length × 25 mm in width, and then, in an environment of 140° C., one end of the second protective sheet of the polarizing sheet is held and peeled off to a length of 10 mm at a speed of 10 mm / min in a direction of 180°, and the adhesion strength of the second protective sheet to the polarizing film, measured when the second protective sheet is peeled off to a length of 10 mm, satisfies the requirement of 40 N / 25 mm or more and 500 N / 25 mm or less.
3. The polarizing sheet according to claim 1 , wherein the polyurethane adhesive is a one-component moisture crosslinking type or a two-component crosslinking type.
4. The polarizing sheet according to claim 3 , wherein the first protective sheet and the second protective sheet are each made mainly of a polycarbonate-based resin or a polyamide-based resin.
5. 5. The polarizing sheet according to claim 1, wherein the polarizing film is made of a polyvinyl alcohol resin or a derivative thereof as a main material, contains a dichroic dye, and is uniaxially stretched.
6. The polarizing sheet according to claim 1, wherein the polarizing sheet is curved so that the first protective sheet forms a concave surface and the second protective sheet forms a convex surface, and the polarizing sheet is placed in a cavity of a mold of an injection molding machine so that the convex side of the polarizing sheet faces the mold of the injection molding machine and the concave side is exposed, and is used to form an optical lens to be joined to the first protective sheet by injection molding, the optical lens being made primarily of an optical resin for injection molding.
7. 7. A polarizing lens comprising: the polarizing sheet according to claim 6, in which the first protective sheet forms a concave surface and the second protective sheet forms a convex surface to form a curved plate; and the optical lens bonded to the first protective sheet on the concave surface and formed by injection molding.
8. 8. The polarized lens according to claim 7, wherein when the haze value of the polarized lens is measured in accordance with JIS K 7136:2000 after immersing the polarized lens in distilled water at 80° C. for 15 minutes, the haze value is 0.05% or more and 1.00% or less.
9. The polarized lens according to claim 7 , wherein when the polarized lens is used, the concave surface of the polarizing sheet facing the first protective sheet faces the user's eyes.
10. 8. The polarizing lens according to claim 7, wherein in the polarizing sheet included in the polarizing lens, the difference between the curve in the MD and the curve in the TD is 0.05 or more and 0.5 or less.
11. An optical component comprising the polarizing lens according to claim 7.
Citation Information
Patent Citations
Polarizing layer laminate and its manufacturing method
JP2009294445A
Cited By
Optical composite molding and production method thereof
EP4810219A1
Polarizing sheet, hot-bent body, sunglasses, and production method for hot-bent body
WO2026211412A1