A preparation method and application of high temperature composite solid electrolyte

By using composite solid electrolytes with PEO, ZrO2 and LiTFSI combined with PAN-UiO66 electrospinning film in lithium metal batteries, the problems of poor ion conductivity and mechanical properties of solid electrolytes are solved, and higher lithium ion transmission efficiency and Battery stability.

CN117913356BActive Publication Date: 2024-12-06HARBIN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410082912.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-19
Publication Date
2024-12-06
Estimated Expiration
2044-01-19

AI Technical Summary

Technical Problem

The poor ionic conductivity and poor mechanical properties of existing solid electrolytes limit the energy density and cycle life of lithium metal batteries.

Method used

Polyethylene oxide (PEO) is used as the polymer substrate, zirconium oxide (ZrO2) is used as the filler, lithium bistrifluoromethanesulfonimide (LiTFSI) is used as the lithium salt, combined with PAN-UiO66 electrospinning film to form a high-temperature composite solid electrolyte , improve the transmission channel and mechanical properties of lithium ions.

Benefits of technology

It significantly improves the conductivity and mechanical properties of lithium ions, extends the cycle life and energy density of lithium metal batteries, and enhances the overall performance of the battery, especially the stability and electrochemical window of lithium ions at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117913356B_ABST
    Figure CN117913356B_ABST
Patent Text Reader

Abstract

A preparation method and application of a high-temperature composite solid electrolyte, which relates to a preparation method and application of a solid electrolyte. The purpose of the invention is to solve the problems of poor ionic conductivity and poor mechanical properties of existing solid electrolytes. The present invention uses PEO as a polymer substrate, ZrO2 as a filler, lithium bis(trifluoromethanesulfonyl imide) as a lithium salt, and PAN-UiO66 electrospinning membrane as a skeleton to prepare a composite solid electrolyte. The spinning skeleton improves the ionic conductivity and mechanical properties of the electrolyte, forming a fast Li + The transmission channel improves the overall performance of the all-solid-state battery. Through the design of the composite structure, the advantages of each component are used to comprehensively improve the cycle performance of the lithium iron phosphate battery. A high-temperature composite solid electrolyte is used in an all-solid-state lithium metal battery. The present invention can obtain a high-temperature composite solid electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method of a solid electrolyte and application thereof. Background Art

[0002] With the development of economy and the improvement of human production and living standards, the demand for energy continues to grow. At present, the energy consumption on the earth mainly relies on petrochemical energy, which has led to serious environmental pollution problems. Therefore, clean, safe and efficient energy has become increasingly important. As we all know, lithium metal batteries have been widely used in mobile electronic devices such as mobile phones, laptops, cameras, etc. due to their advantages such as high operating voltage, large energy density and long cycle life. Recent research work has focused on methods to give lithium metal batteries higher energy density and longer cycle life at a lower cost. However, traditional organic liquid lithium ion electrolytes have safety issues such as volatility and poor chemical stability, resulting in low coulombic efficiency, short circuit and catastrophic failure of the battery. Compared with traditional lithium ion batteries, solid-state lithium metal batteries have higher energy density, longer cycle life and better safety.

[0003] Polyethylene oxide (PEO) has good chemical compatibility with lithium anode, good flexibility and easy processing. At high temperature, the polymer chain segments in the PEO-based all-solid electrolyte move and move, quickly transporting lithium ions in the absence of any liquid, and the ion conductivity is usually 10 –4 -10 –7 Scm –1 In this range, higher ionic conductivity can generally be obtained by increasing the content of lithium salt in the electrolyte (EO:Li).

[0004] However, its main disadvantages are poor ionic conductivity and poor mechanical properties. Summary of the invention

[0005] The purpose of the present invention is to solve the problems of poor ion conductivity and poor mechanical properties of existing solid electrolytes, and to provide a preparation method and application of a high-temperature composite solid electrolyte.

[0006] The present invention uses PEO as a polymer substrate, ZrO2 as a filler, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) as a lithium salt, and PAN-UiO66 electrospinning membrane as a skeleton to prepare a composite solid electrolyte. The spinning skeleton improves the ionic conductivity and mechanical properties of the electrolyte, forming a fast Li + The transmission channel improves the overall performance of all-solid-state batteries. Through the design of the composite structure, the advantages of each component are used to comprehensively improve the cycle performance of lithium iron phosphate (LFP) batteries.

[0007] A method for preparing a high-temperature composite solid electrolyte is specifically completed by the following steps:

[0008] 1. Preparation of PAN-UiO66 electrospinning membrane:

[0009] ① First, disperse polyacrylonitrile and metal organic framework into an organic solvent, ultrasonicate for a period of time, and then stir to obtain a uniform spinning precursor solution;

[0010] ②, loading a uniform spinning precursor solution into a syringe and performing electrospinning in a spinning machine;

[0011] ③, peel off the spun fiber membrane from the drum collector and place it in a vacuum drying oven for vacuum drying for a period of time, cool it to room temperature, and obtain the PAN-UiO66 electrospun membrane;

[0012] 2. Preparation of polymer solid electrolyte:

[0013] PEO, LiTFSI and ZrO2 were dissolved in acetonitrile, ultrasonicated for a period of time, and then magnetically stirred to obtain a mixed solution;

[0014] 3. Place the PAN-UiO66 electrospun membrane on a pre-cleaned polytetrafluoroethylene plastic plate, pour the mixed solution on the PAN-UiO66 electrospun membrane, and then vacuum dry it. Peel the dried membrane off the polytetrafluoroethylene plastic plate and vacuum dry it again to obtain a high-temperature composite solid electrolyte.

[0015] A high-temperature composite solid electrolyte is used in all-solid-state lithium metal batteries.

[0016] Principle of the present invention:

[0017] Inorganic fillers can increase the Lewis acid-base sites in the electrolyte, strengthen the interaction between polymer segments and lithium ions, and improve the ionic conductivity of the solid electrolyte. In addition, inorganic fillers and electrospinning support membranes can reduce the crystallinity of polymer solid electrolytes and provide good mechanical properties. In the present invention, zirconium oxide (ZrO2) has a higher band gap, can broaden the molecular orbital energy level of the composite electrolyte, increase the electrochemical stability of the electrolyte, provide Lewis acid sites in the electrolyte, and is conducive to the complexation and decomplexation of lithium salts; it has high electrochemical and thermal stability; polyacrylonitrile (PAN) has high oxidation resistance and stability, and has an electron-withdrawing nitrile group (-CN), which can compete with the ether oxygen bond (-O-) in PEO for lithium ions, accelerating the complexation and decomplexation of lithium ions during transportation. The organic metal framework (UiO-66MOF) is an octahedral structure nanomaterial centered on zirconium atoms, which can be evenly dispersed in PAN to prepare an electrospinning support membrane with high mechanical strength.

[0018] Advantages of the present invention:

[0019] The electrochemical properties of the composite all-solid electrolyte and the polymer all-solid electrolyte were compared with or without the addition of PAN-UiO66 electrospinning membrane. The results showed that the addition of PAN-UiO66 electrospinning membrane increased the ionic conductivity of the composite all-solid electrolyte from 1.94×10 –4 Scm –1 Increased to 2.50×10 –4 Scm –1 , the lithium ion migration number increased from 0.20 to 0.40, and the electrochemical voltage window increased from 4.58 V to 5.10 V; in addition, the addition of PAN-UiO66 electrospinning membrane enabled the Li||Li symmetric battery assembled with composite all-solid electrolyte to achieve a charge transfer rate of 0.1 mA cm -2 The assembled LFP||Li button-type full cell has a capacity of 149.81 mAh g at a current density of 0.5 C. –1 The discharge specific capacity of the battery is 101.53% after 200 cycles, which reflects the development potential of composite solid electrolytes. The assembled LFP||Li soft-pack battery has a capacity retention rate of 113.21 mAh g at a rate of 0.5 C. –1 The discharge specific capacity has a capacity retention rate of 86.7% after 100 cycles. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 are SEM images, in which (a) is the PAN-UiO66 electrospinning membrane prepared in step 1 of Example 1, (b) is the surface SEM image of the polymer electrolyte PZ prepared in comparative example 1, and (c) is the surface SEM image of the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1;

[0021] Figure 2 Ionic conductivity of the polymer electrolyte PZ prepared in Comparative Example 1 and the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1 at high temperature;

[0022] Figure 3 At 0.1mVs -1 Electrochemical voltage window curves of the polymer electrolyte PZ prepared in Comparative Example 1 and the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1 at a scan rate of ;

[0023] Figure 4 The chronoamperometric curve of a lithium symmetric battery assembled using the polymer electrolyte PZ prepared in Comparative Example 1 and the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1;

[0024] Figure 5The electrochemical impedance spectra of a lithium symmetric battery assembled using the polymer electrolyte PZ prepared in Comparative Example 1 and the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1 were tested before and after polarization at room temperature;

[0025] Figure 6 The critical current density curve of the lithium symmetric battery Li / PZ / Li assembled using the polymer electrolyte PZ prepared in Comparative Example 1;

[0026] Figure 7 The critical current density curve of the lithium symmetric battery Li / PZPU / Li assembled using the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1;

[0027] Figure 8 At 0.1mAcm -2 At a current density of , constant current cycle curves of a lithium symmetric battery Li / PZ / Li assembled using the polymer electrolyte PZ prepared in Comparative Example 1 and a lithium symmetric battery Li / PZPU / Li assembled using the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1;

[0028] Fig. 9 The rate performance curves of the LFP / PZ / Li full battery assembled using the polymer electrolyte PZ prepared in Comparative Example 1 and the LFP / PZPU / Li full battery assembled using the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1 at different current densities;

[0029] Fig.10 Cycling performance curves of an LFP / PZ / Li full battery assembled with the polymer electrolyte PZ prepared in Comparative Example 1 and an LFP / PZPU / Li full battery assembled with the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1 at a rate of 0.5C;

[0030] Fig.11 The electrochemical performance curve of the LFP / PZPU / Li full battery assembled with the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1 at a rate of 0.5C. DETAILED DESCRIPTION

[0031] Specific implementation method 1: This implementation method is a method for preparing a high-temperature composite solid electrolyte, which is specifically completed according to the following steps:

[0032] 1. Preparation of PAN-UiO66 electrospinning membrane:

[0033] ① First, disperse polyacrylonitrile and metal organic framework into an organic solvent, ultrasonicate for a period of time, and then stir to obtain a uniform spinning precursor solution;

[0034] ②, loading a uniform spinning precursor solution into a syringe and performing electrospinning in a spinning machine;

[0035] ③, peel off the spun fiber membrane from the drum collector and place it in a vacuum drying oven for vacuum drying for a period of time, cool it to room temperature, and obtain the PAN-UiO66 electrospun membrane;

[0036] 2. Preparation of polymer solid electrolyte:

[0037] PEO, LiTFSI and ZrO2 were dissolved in acetonitrile, ultrasonicated for a period of time, and then magnetically stirred to obtain a mixed solution;

[0038] 3. Place the PAN-UiO66 electrospun membrane on a pre-cleaned polytetrafluoroethylene plastic plate, pour the mixed solution on the PAN-UiO66 electrospun membrane, and then vacuum dry it. Peel the dried membrane off the polytetrafluoroethylene plastic plate and vacuum dry it again to obtain a high-temperature composite solid electrolyte.

[0039] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that: the metal organic framework described in step 1① is UiO-66; the organic solvent described in step 1① is N,N-dimethylformamide; the mass ratio of the metal organic framework described in step 1① to polyacrylonitrile is (0.1-0.15):1. The other steps are the same as those in specific embodiment 1.

[0040] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that: the ultrasonic temperature in step 1① is 25℃~40℃, and the ultrasonic time is 1h~3h; the stirring time in step 1① is 12h~24h; the concentration of polyacrylonitrile in the uniform spinning precursor solution in step 1① is 5%~15%. The other steps are the same as those in specific implementation method 1 or 2.

[0041] Specific embodiment 4: The difference between this embodiment and specific embodiments 1 to 3 is that the voltage of the electrospinning described in step 1② is 16kV to 20kV, and the feed rate is 0.5mLh -1 ~1mLh -1 The distance between the syringe needle and the collector is 15 cm to 20 cm, the rotating speed of the collector is 300 r / min to 500 r / min, and the humidity is set to 30% to 40% at room temperature. The other steps are the same as those of the first to third embodiments.

[0042] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that the vacuum drying temperature in step 1③ is 60°C to 80°C and the vacuum drying time is 12h to 24h. The other steps are the same as those in specific embodiments 1 to 4.

[0043] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that the mass ratio of PEO to LiTFSI in step 2 is 8:1; the mass ratio of ZrO2 to PEO in step 2 is (5-10): 100. The other steps are the same as those in specific embodiments 1 to 5.

[0044] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that: the ultrasonic time in step 2 is 1h to 3h; the magnetic stirring time in step 2 is 24h to 36h; the concentration of PEO in the mixed solution in step 2 is 5% to 10%. The other steps are the same as those in specific embodiments 1 to 6.

[0045] Specific embodiment eight: The difference between this embodiment and specific embodiments one to seven is that the vacuum drying temperature in step three is 60°C to 80°C, and the vacuum drying time is 12h to 24h;

[0046] The volume ratio of the mixed solution described in step 3 to the surface area of ​​the PAN-UiO66 electrospinning membrane is (30 mL to 60 mL): (20 cm 2 ~50cm 2 ). The other steps are the same as those in Specific Embodiments 1 to 7.

[0047] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that the thickness of the high-temperature composite solid electrolyte in step 3 is 80 μm to 150 μm. The other steps are the same as those in specific embodiments 1 to 8.

[0048] Specific implementation method ten: This implementation method is an application of a high-temperature composite solid electrolyte in an all-solid-state lithium metal battery.

[0049] The following examples are used to verify the beneficial effects of the present invention:

[0050] Example 1: A method for preparing a high-temperature composite solid electrolyte is specifically completed by the following steps:

[0051] 1. Preparation of PAN-UiO66 electrospinning membrane:

[0052] ① First, polyacrylonitrile (PAN) and UiO-66 were dispersed in N,N-dimethylformamide, ultrasonicated at 25°C for 1 hour, and then stirred at a stirring speed of 500 r / min for 12 hours to obtain a uniform spinning precursor solution;

[0053] The mass ratio of UiO-66 to polyacrylonitrile described in step 1① is 0.1:1;

[0054] The concentration of polyacrylonitrile in the uniform spinning precursor solution described in step 1① is 10%;

[0055] ②, loading a uniform spinning precursor solution into a syringe and performing electrospinning in a spinning machine;

[0056] The voltage of the electrospinning described in step 1② is 16 kV, and the feed rate is 0.5 mL / h -1 , the distance between the syringe needle and the collector was 15 cm, the rotation speed of the collector was 300 r / min, and the humidity was set to 30% at room temperature;

[0057] ③, peel off the spun fiber membrane from the drum collector and place it in a vacuum drying oven at 60°C for 12 hours, and cool it to room temperature to obtain a PAN-UiO66 electrospun membrane;

[0058] 2. Preparation of polymer solid electrolyte:

[0059] PEO, LiTFSI and ZrO2 were dissolved in acetonitrile, ultrasonicated for 1 h, and then magnetically stirred for 24 h to obtain a mixed solution;

[0060] The mass ratio of PEO and LiTFSI described in step 2 is 8:1;

[0061] The mass ratio of ZrO2 to PEO described in step 2 is 5:100;

[0062] The concentration of PEO in the mixed solution described in step 2 is 10%;

[0063] 3. Place the PAN-UiO66 electrospun membrane on a pre-cleaned polytetrafluoroethylene plastic plate, cast the mixed solution on the PAN-UiO66 electrospun membrane, and then vacuum dry it in a vacuum drying oven at 60°C for 24 hours, peel off the dried membrane from the polytetrafluoroethylene plastic plate, and then vacuum dry it in a vacuum drying oven at 60°C for 12 hours to obtain a high-temperature composite solid electrolyte (PZPU);

[0064] The volume ratio of the mixed solution described in step 3 to the surface area of ​​the PAN-UiO66 electrospinning membrane is 50 mL:40 cm 2 ;

[0065] The thickness of the high-temperature composite solid electrolyte described in step three is 100 μm.

[0066] Comparative Example 1: The preparation method of polymer electrolyte PZ is specifically completed according to the following steps:

[0067] 1. PEO, LiTFSI and ZrO2 were dissolved in acetonitrile, ultrasonicated for 1 h, and then magnetically stirred for 24 h to obtain a mixed solution;

[0068] The mass ratio of PEO and LiTFSI described in step 1 is 8:1;

[0069] The mass ratio of ZrO2 to PEO described in step 1 is 5:100;

[0070] The concentration of PEO in the mixed solution described in step 1 is 10%;

[0071] 2. Cast the mixed solution on a pre-cleaned polytetrafluoroethylene plastic plate, and then vacuum dry it in a vacuum drying oven at 60°C for 24 hours, peel off the dried film from the polytetrafluoroethylene plastic plate, and then vacuum dry it in a vacuum drying oven at 60°C for 12 hours to obtain a polymer electrolyte (PZ);

[0072] The thickness of the high temperature composite solid electrolyte described in step 2 is 100 μm.

[0073] Figure 1 are SEM images, in which (a) is the PAN-UiO66 electrospinning membrane prepared in step 1 of Example 1, (b) is the surface SEM image of the polymer electrolyte PZ prepared in comparative example 1, and (c) is the surface SEM image of the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1;

[0074] from Figure 1 In (a), it can be observed that the prepared PAN-UiO66 electrospun membrane has uniform pores and the fiber diameter is about 300nm. Figure 1 (b) It can be observed that the PZ surface is very rough, the polymer is severely agglomerated, and there are many defects, which are not conducive to the stable transport of lithium ions; Figure 1 (c) It can be observed that the prepared PZPU surface has a uniform morphology and a smooth surface, indicating that the addition of PAN-UiO66 electrospinning membrane improves the polymer crystallinity. The smooth surface morphology helps to achieve good contact between the electrolyte and the electrode, improves the interfacial properties of the solid electrolyte, and enhances the rapid transfer of lithium ions.

[0075] Figure 2 Ionic conductivity of the polymer electrolyte PZ prepared in Comparative Example 1 and the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1 at high temperature;

[0076] from Figure 2 It can be seen that after adding PAN-UiO66 electrospinning membrane, the ionic conductivity of the solid electrolyte increased from 1.94×10 – 4 Scm –1 Increased to 2.50×10 –4 Scm –1The higher ionic conductivity is due to the fact that the PAN-UiO66 electrospinning membrane reduces the crystallinity of the composite electrolyte, and the electron-withdrawing -CN groups in PAN and the ether oxygen bonds in PEO compete for lithium ions, increasing the solubility of lithium salts and thus increasing the ionic conductivity.

[0077] Figure 3 At 0.1mVs -1 Electrochemical voltage window curves of the polymer electrolyte PZ prepared in Comparative Example 1 and the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1 at a scan rate of ;

[0078] Figure 3 The electrochemical stability windows of the prepared PZ and PZPU electrolytes were determined by using linear sweep voltammetry curves. When the maximum current was set to 10 μA, the stable electrochemical voltage window of the polymer PZ membrane was limited to 4.58 V, while the working voltage of the PZPU membrane increased to 5.10 V. The high voltage tolerance of the PZPU membrane may be due to the fact that the PAN-UiO66 electrospinning membrane broadened the molecular orbital energy levels of the composite electrolyte and improved the stability of the composite electrolyte under high voltage.

[0079] Assembling lithium symmetrical batteries: The preparation method of Li|PU|Li and Li|PZPU|Li is as follows: first prepare a negative electrode shell, place a spring, place a gasket, place a 14mm lithium sheet, place PZ and PZPU electrolytes respectively, and then place a 14mm lithium sheet, then cover the positive electrode shell, and put it into a button battery packaging machine to complete the packaging.

[0080] Figure 4 The chronoamperometric curve of a lithium symmetric battery assembled using the polymer electrolyte PZ prepared in Comparative Example 1 and the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1;

[0081] Figure 5 The electrochemical impedance spectra of a lithium symmetric battery assembled using the polymer electrolyte PZ prepared in Comparative Example 1 and the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1 were tested before and after polarization at room temperature;

[0082] Calculations show that by adding PAN-UiO66 electrospinning membrane, the lithium ion migration number increases from 0.20 to 0.40, the segmental motion of the polymer chain is enhanced due to the lower crystallinity, and the PAN-UiO66 electrospinning membrane blocks the larger TFSI to a certain extent. - The results of anions.

[0083] Figure 6 The critical current density curve of the lithium symmetric battery Li / PZ / Li assembled using the polymer electrolyte PZ prepared in Comparative Example 1;

[0084] Figure 7 The critical current density curve of the lithium symmetric battery Li / PZPU / Li assembled using the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1;

[0085] from Figure 6 and Figure 7 It can be seen that the critical current density of the lithium symmetric battery Li / PZ / Li assembled using the polymer electrolyte PZ prepared in Comparative Example 1 is 0.25 mA cm -2 After adding PAN-UiO66 electrospinning membrane, the critical current density increased to 0.35 mA cm -2 , which reflects the good compatibility of PZPU with lithium metal and its inhibitory effect on lithium dendrites.

[0086] By using a symmetrical lithium battery and 0.1mAcm -2 The interfacial stability of the prepared electrolyte membrane and Li metal electrode was evaluated by cycling at a current density of . Figure 8 It shows that the Li / PZPU / Li symmetric battery provides more than 670h of stable and uninterrupted cycling during electroplating and stripping, while the Li / PZ / Li symmetric battery gradually short-circuits after cycling for more than 230h. In addition, compared with the Li / PZ / Li symmetric battery, the average polarization voltage of the Li / PZPU / Li symmetric battery is also much smaller (~100mV). This shows that the PAN-UiO66 electrospinning membrane effectively improves the interfacial contact between PZPU and lithium metal, and the high mechanical strength inhibits the growth of lithium dendrites during the cycle.

[0087] Assembling the full battery: The preparation method of LFP|PU|Li and LFP|PZPU|Li is as follows: first prepare a negative electrode shell, place a spring, place a gasket, place a 14mm lithium sheet, place PZ and PZPU electrolytes respectively, and then place 12mm lithium iron phosphate (LFP), then cover the positive electrode shell, and put it into the button battery packaging machine to complete the packaging.

[0088] By using a symmetrical lithium battery and 0.1mAcm -2 The interfacial stability of the prepared electrolyte membrane and Li metal electrode was evaluated by cycling at a current density of .

[0089] Figure 8 At 0.1mAcm -2 At a current density of , constant current cycle curves of a lithium symmetric battery Li / PZ / Li assembled using the polymer electrolyte PZ prepared in Comparative Example 1 and a lithium symmetric battery Li / PZPU / Li assembled using the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1;

[0090] Figure 8It shows that the Li / PZPU / Li symmetric battery provides more than 670h of stable and uninterrupted cycling during electroplating and stripping, while the Li / PZ / Li symmetric battery gradually short-circuits after cycling for more than 230h. In addition, compared with the Li / PZ / Li symmetric battery, the average polarization voltage of the Li / PZPU / Li symmetric battery is also much smaller (~100mV). This shows that the PAN-UiO66 electrospinning membrane effectively improves the interfacial contact between PZPU and lithium metal, and the high mechanical strength inhibits the growth of lithium dendrites during the cycle.

[0091] Rate performance curves of LFP / PZ / Li and LFP / PZPU / Li full cells at different current densities (0.1C, 0.2C, 0.5C, 1C), following a procedure of five charge and discharge cycles at room temperature, see Fig. 9 As shown;

[0092] Fig. 9 The rate performance curves of the LFP / PZ / Li full battery assembled using the polymer electrolyte PZ prepared in Comparative Example 1 and the LFP / PZPU / Li full battery assembled using the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1 at different current densities;

[0093] from Fig. 9 It can be seen that the initial discharge capacities of LFP / PZPU / Li batteries at 0.1C, 0.2C, 0.5C and 1C are 154.53, 152.38, 135.24 and 114.10 mAh g, respectively. -1 Compared with LFP / PZ / Li batteries (152.55, 145.80, 115.97 and 40.31 mAhg -1 ) has a higher discharge specific capacity.

[0094] Fig.10 Cycling performance curves of an LFP / PZ / Li full battery assembled with the polymer electrolyte PZ prepared in Comparative Example 1 and an LFP / PZPU / Li full battery assembled with the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1 at a rate of 0.5C;

[0095] Fig.10 Comparison of the charge / discharge cycle performance of LFP / PZ / Li and LFP / PZPU / Li button cells at 0.5C is shown. The LFP / PZPU / Li full cell exhibits 149.18 mAh g -1 The initial discharge capacity of the battery can be maintained at 101.53% after 200 cycles. –1, the battery basically failed after 70 cycles). The improved cycle stability and capacity retention rate of LFP / PZPU / Li battery may be due to the high mechanical strength PAN-UiO66 electrospinning membrane improving the stability of the electrolyte and reducing the crystallinity of the polymer electrolyte, thereby achieving rapid and stable transport of lithium ions.

[0096] Fig.11 The electrochemical performance curve of the LFP / PZPU / Li full battery assembled with the high-temperature composite solid electrolyte PZPU prepared in step 3 of Example 1 at a rate of 0.5C.

[0097] Fig.11 The LFP / PZPU / Li full-cell battery shows the charge / discharge cycle performance at 0.5C. The LFP / PZPU / Li full-cell battery shows 113.21mAhg -1 The initial discharge capacity of LFP / PZPU / Li battery has a capacity retention rate of 86.7% after 100 cycles. The high cycle stability and capacity retention rate of LFP / PZPU / Li battery indicate that the composite electrolyte can be prepared on a large scale, accelerating the commercialization process of all-solid-state electrolytes.

Claims

1. A method for preparing a high-temperature composite solid electrolyte, Features The ionic conductivity of the high-temperature composite solid electrolyte prepared by the preparation method is 2.50×10 –4 Scm –1 , the lithium ion transfer number is 0.40, the electrochemical voltage window is 5.10V, and the Li / PZPU / Li symmetric battery assembled with the high temperature composite solid electrolyte has a high conductivity at 0.1mAcm -2 The assembled LFP / PZPU / Li full cell exhibited a stable electroplating and stripping performance for more than 670 h at a current density of 0.5 C and a high capacity of 149.81 mAh g –1 The discharge specific capacity has a capacity retention rate of 101.53% after 200 cycles; the preparation method is specifically completed according to the following steps:

1. Preparation of PAN-UiO66 electrospinning membrane: ① First, disperse polyacrylonitrile and UiO-66 in N,N-dimethylformamide, ultrasonicate for 1 h at 25 °C, and then stir for 12 h at a stirring speed of 500 r / min to obtain a uniform spinning precursor solution; The mass ratio of UiO-66 to polyacrylonitrile described in step 1① is 0.1:1; The concentration of polyacrylonitrile in the uniform spinning precursor solution described in step 1① is 10%; ②, loading a uniform spinning precursor solution into a syringe and performing electrospinning in a spinning machine; The voltage of the electrospinning described in step 1② is 16 kV, and the feed rate is 0.5 mL / h -1 , the distance between the syringe needle and the collector was 15 cm, the rotation speed of the collector was 300 r / min, and the humidity was set to 30% at room temperature; ③, peeling off the spun fiber membrane from the drum collector and placing it in a vacuum drying oven at a temperature of 60°C for vacuum drying for 12 hours, cooling it to room temperature, and obtaining a PAN-UiO66 electrospun membrane; 2. Preparation of polymer solid electrolyte: PEO, LiTFSI and ZrO 2 Dissolve in acetonitrile, sonicate for 1 h, and then magnetically stir for 24 h to obtain a mixed solution; The mass ratio of PEO and LiTFSI described in step 2 is 8:1; The ZrO 2 The mass ratio with PEO is 5:100; The concentration of PEO in the mixed solution described in step 2 is 10%; 3. Place the PAN-UiO66 electrospun membrane on a pre-cleaned polytetrafluoroethylene plastic plate, cast the mixed solution on the PAN-UiO66 electrospun membrane, and then vacuum dry it in a vacuum drying oven at 60°C for 24 hours, peel off the dried membrane from the polytetrafluoroethylene plastic plate, and then vacuum dry it in a vacuum drying oven at 60°C for 12 hours to obtain a high-temperature composite solid electrolyte, recorded as PZPU; The volume ratio of the mixed solution described in step 3 to the surface area of ​​the PAN-UiO66 electrospinning membrane is 50 mL:40 cm 2 ; The thickness of the high-temperature composite solid electrolyte described in step three is 100 μm.