A method for preparing polymer capsules
Polymer capsules were prepared by grafting high molecular weight monomers and microfluidic control technology, combined with CT scanning and image processing technology, and solved the problems of high injection pressure and viscosity loss of traditional polymer flooding in low permeability reservoirs, achieving the following: High-efficiency oil displacement effect in medium and low permeability reservoirs.
Patent Information
- Application Number
- CN202410324012.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-21
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-03-21
AI Technical Summary
Traditional polymer flooding has challenges such as high injection pressure and high viscosity loss in the development of low-permeability reservoirs. There is a lack of tools to visualize the microscopic seepage mechanism in simulated actual formation environments, which affects the oil flooding effect.
The polymer capsules were prepared by chemical grafting and microfluidic control methods, and the CT scanning and image processing technology were used to accurately locate and study their migration and adsorption in the core. Deformation sealing, rupture and diffusion mechanism.
The precise positioning and microscopic seepage mechanism of polymer capsules in actual formation environments are achieved, which enhances the oil repellent effect and improves the oil repellent performance of polymer capsules through slow release characteristics.
Smart Images

Figure CN117924751B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a polymer capsule, and belongs to the technical field of oil and gas field development engineering. Background Art
[0002] In oilfield exploitation, polymer flooding is one of the most commonly used oil recovery methods. Polymers can increase the viscosity of the displacement phase, improve the oil-water mobility ratio, and expand the swept volume of the injected water, thereby improving the displacement efficiency. With the continuous development of oil resources, the research and practice of developing medium and low permeability reservoirs has attracted increasing attention. However, due to its low porosity and low permeability characteristics, traditional polymer flooding, especially high viscoelastic polymer flooding, faces severe challenges, such as high injection pressure and large viscosity loss.
[0003] In order to improve the injectability of polymers, the concept of delayed viscosity increase was proposed, aiming to transfer the viscosity increase process from the ground to the displacement process of the reservoir. In recent years, microcapsules have gradually been used in various fields such as biomedicine, food, self-healing materials and cosmetics due to their unique slow release characteristics. Microcapsules encapsulate polymers in shells through encapsulation to form particles with a core-shell structure, effectively isolating the internal core material from the external environment, and achieving precise control of the protection and release of the core material.
[0004] Microcapsules are also used as additives in the field of oil development and have potential economic value. However, there are currently few microcapsules that can be visualized for research under simulated formation conditions. There is an urgent need to develop a polymer capsule that can be used to visualize the microscopic seepage mechanism in a simulated actual formation environment. The density of the polymer capsule can be adjusted according to academic research or actual displacement needs, but regardless of the specific value of the density, it can effectively enhance the oil recovery effect, so as to deeply explore its key mechanisms such as migration adsorption, deformation plugging, and fracture diffusion. It not only provides a flexible and highly controllable research tool for the academic community, but also provides a feasible and economical solution for practical applications. Summary of the invention
[0005] In view of the shortcomings of the prior art, in order to generate polymer capsules grafted with high molecular weight monomers, accurately study the microscopic seepage mechanisms of polymer capsules in actual formation environments, such as migration and adsorption mechanism, deformation and plugging mechanism, fracture and diffusion mechanism, and study the relationship between these seepage mechanisms and oil recovery effect, the present invention provides a method for preparing polymer capsules.
[0006] The technical solution of the present invention is as follows:
[0007] A method for preparing a polymer capsule comprises the following steps:
[0008] (1) Measure the density of rock particles and the density of the displaced phase;
[0009] (2) Selecting an original high-viscoelastic polymer and a high molecular weight monomer, measuring the density of the original polymer solution, and setting the mixing ratio of the original polymer and the high molecular weight monomer according to the density difference between the original polymer solution and the rock particles and the displaced phase; synthesizing a high-density target polymer grafted with a high molecular weight monomer as a core material by chemical grafting;
[0010] (3) Preparation of polymer capsules by microfluidics;
[0011] (4) The prepared polymer capsules are formulated into a solution and injected into a core saturated with oil. A core slice image is obtained by CT scanning. The grayscale value ranges of the polymer capsules, rock particles and crude oil in the scanned image are determined by image processing software. If the grayscale value ranges of the polymer capsules, rock particles and crude oil overlap by more than 10%, the process returns to step (2), adjusts the mixing ratio of the original polymer and the high molecular weight monomer, and re-prepares the polymer capsules.
[0012] Preferably, in step (1), the rock density is measured using nuclear magnetic resonance technology. The conventional rock density is 2.2-2.8 g / cm 3 The density of the displaced phase is measured using a densitometer. The displaced phase is crude oil, and the density of conventional crude oil is 0.8-0.95 g / cm 3 The density of the polymer solution used is measured by a densitometer.
[0013] Preferably, in step (2), the original polymer is one of polyacrylamide, polyvinylamide, sulfonated polyacrylic acid, sulfonated polyacrylamide, acrylic acid-sulfonated acrylic acid polymer, sulfonated polyvinyl alcohol, and sulfonated polyethylene.
[0014] Preferably, in step (2), the high molecular weight monomer is one of brominated phenol, isobutyl methacrylate, and vinyl dimethoxy silane.
[0015] Preferably, in step (2), the method for preparing the target polymer comprises the following steps:
[0016] (2-1) According to the density difference between the original polymer solution and the rock particles and the displaced phase, the mixing ratio of the original polymer and the high molecular weight monomer is adjusted, and the ratio varies in the range of 1:1-1:10;
[0017] (2-2) Add 0.1%-2% of inorganic catalyst according to the ratio. The higher the proportion of high molecular weight monomer, the greater the amount of inorganic catalyst added. The mass ratio of original polymer, high molecular weight monomer and inorganic catalyst is 1: (0.02-0.2): (0.002-0.1);
[0018] (2-3) The entire preparation was carried out under a nitrogen atmosphere, at a temperature range of 65–85 °C and stirred at 500 r / min for 4–9 h.
[0019] Preferably, in step (2-1), the mass fraction of the polymer in the original polymer solution is 40-60%.
[0020] Preferably, in step (2-2), the inorganic catalyst is one of hydrogen peroxide, ammonium persulfate, peracetic acid, and ethyl peroxide.
[0021] Preferably, in step (3), the wall material of the polymer capsule is composed of cellulose nanocrystal-alginate hydrogel, which is dispersed at 500 r / min for 4-6 h, with a cellulose nanocrystal content in the range of 0.05wt%-0.3wt% and an alginate content in the range of 1%-6%.
[0022] Further preferably, in step (3), the cellulose nanocrystals have a length of 100-200 nm and a diameter of 3-20 nm, and the alginate is one of sodium alginate, calcium galacturonate, carrageenan and guara gum.
[0023] Preferably, in step (3), the polymer capsule is synthesized using a microfluidic device, the microfluidic device comprising three microdisplacement systems and a co-flow and confocal combination capillary, the three microdisplacement systems are respectively microdisplacement system A, microdisplacement system B, and microdisplacement system C, each microdisplacement system comprises a microdisplacement pump, a microinjector, and a catheter, an injection capillary and a collection capillary are arranged in the co-flow and confocal combination capillary, the injection capillary and the collection capillary both comprise a cone with a reduced inner diameter, the injection capillary and the collection capillary are arranged at their minimum openings relative to each other, a channel 1 is formed in the injection capillary, a channel 2 is formed between the collection capillary and the inner wall of the co-flow and confocal combination capillary, and a channel 3 is formed between the injection capillary and the inner wall of the co-flow and confocal combination capillary;
[0024] The preparation method comprises the following steps:
[0025] (3-1) The target polymer is contained in the micro-displacement system A as the core material and is injected from channel one; the cellulose nanocrystal-alginate hydrogel is contained in the micro-displacement system B as the wall material and is injected from channel two; the organic solution is contained in the micro-displacement system C as the intermediate phase and is injected from channel three, and the organic solution is one of ethanol, isopropanol, undecanol, dodecanol, benzyl alcohol, octanol, ethylene glycol dimethyl ether, ethylene glycol methyl ether, acetone, methyl tert-butyl ketone, ethyl acetate, butanone, toluene, and xylene;
[0026] (3-2) adjusting the flow rate range of the target polymer and the cellulose nanocrystals, wherein the injection flow rate of the target polymer varies in the range of 1-100 μL / min, and the injection flow rate of the cellulose nanocrystals varies in the range of 100-1000 μL / min, to generate a stable emulsion polymer;
[0027] (3-3) placing the generated emulsion polymer in a solution containing a cross-linking agent for stabilization for 2-4 hours to form a hydrogel shell, wherein the cross-linking agent is one of aluminum sulfate, calcium chloride, calcium nitrate, ammonium chloride, ferric nitrate, and aluminum chloride;
[0028] (3-4) curing the shell of the polymer capsule by ultraviolet light irradiation to form stable polymer capsule particles;
[0029] (3-5) Wash the polymer capsules twice with distilled water and ethanol respectively;
[0030] (3-6) After being placed in an oven at 35 °C for 24 h, pure and dry polymer capsule particles were obtained.
[0031] Preferably, in step (4), the calculation formula of the overlap degree is as shown in formula (1):
[0032] (1)
[0033] in: d is the overlap between range 1 and range 2, %; a is the length of range 1; b is the length of range 2, c It is the length of the overlap between range 1 and range 2. Range 1 and range 2 refer to the grayscale value ranges for which the overlap degree needs to be calculated.
[0034] Preferably, in step (4), the method comprises:
[0035] Step 1: Inject the prepared polymer capsule into the sand-filled tube or the actual core of the test system. The test system includes a displacement pump, a fluid injection and pressure control acquisition device, and a lead box. A stage is provided in the lead box. A clamp is provided on the stage. The clamp may be a sand-filled tube type clamp or a core clamp. An X-ray source, a CCD camera, and a detector are provided around the clamp. The X-ray source is connected to the CT scanning main console outside the lead box. The clamp is connected to the displacement pump outside the lead box. The fluid injection and pressure control acquisition device is connected to the displacement pump. A temperature sensor is provided on the clamp.
[0036] Step 2: Use the CT scanning console to create a sand-fill tube or actual core slice;
[0037] Step 3: Filter and sharpen the scanned images, and segment the rock phase, pore phase, polymer capsule phase and pure water phase according to the grayscale values of different phases. Use 3D core reconstruction technology to construct a digital core. Since there is a large density difference between polymer capsules and rock, oil phase and pure water phase, the polymer capsule phase can be accurately analyzed. Combined with the 3D digital core, the state of polymer capsules between the core pores can be studied more three-dimensionally. By injecting different amounts of solution into the same core, the displacement channel inside the core is studied, the distribution of polymer capsules is located, and the migration law of polymer capsules is presented in 3D visualization. Then, the displacement of crude oil and the change in the distribution of polymer capsules at the same position are studied, and the oil displacement mechanism of polymer capsules is analyzed.
[0038] Preferably, the test system further includes one of the following solutions:
[0039] a. The test system is also equipped with a temperature control box, which is connected to the displacement pump to control the temperature of the liquid in the displacement pump;
[0040] b. A conversion platform is provided above the stage, a moving platform is provided below the stage, the conversion platform is provided with a screw interface, and the clamp is connected to the conversion platform through the screw interface; it is convenient for fixing and replacement;
[0041] c. A wire collection box is provided in the lead box, which includes a shell, a fixed column is provided in the shell, a wire reel is provided through the fixed column, and springs are provided on the fixed columns at both ends of the wire reel. The pipelines in the lead box are wound around the wire reel; the wire collection box is used to collect the pipelines in the lead box neatly;
[0042] d. The clamp includes a fixed tube, the core is arranged in the fixed tube through a rubber sleeve, a displacement inlet, a confining pressure inlet, a displacement outlet, and a confining pressure outlet are respectively arranged at both ends of the fixed tube, a temperature sensor is respectively arranged at both ends of the fixed tube, and one end of the fixed tube is connected to a waste liquid tank.
[0043] Preferably, in step 1, the sand-filled tube or the core is first vacuumed and saturated with simulated formation water to calculate the porosity and permeability of the sand-filled tube or the core model. The formulas for the permeability and porosity of the sand-filled tube or the core model are shown in equations (2) and (3):
[0044] (2)
[0045] in: k - Permeability of sand packs or core models, ; Q - In pressure difference Flow rate through sand-filled tube or core model, cm 3 / s; A - Cross-sectional area of sand filling tube or core model sand, cm 2 ;L - Length of sand filling tube or core model sand, cm; -Viscosity of the injected fluid, mPa·s; - Pressure difference before and after the fluid passes through the sand packing tube or core model, 10 5 Pa;
[0046] (3)
[0047] in: -Porosity of sand packs or core models; V 孔 - Pore volume of sandfill or core model, obtained by weighing, cm 3 ; A - Cross-sectional area of sand filling tube or core model sand, cm 2 ; L - Length of sand filling tube or core model sand, cm;
[0048] Then, the micropolymer capsules are loaded into the displacement pump, the confining pressure fluid is injected, the confining pressure and its temperature are measured, and when the temperature detected by the temperature sensor reaches the formation temperature and the pressure in the fluid injection and pressure control acquisition device reaches the formation pressure range, the displacement pump is turned on, the flow rate is set to 1 μL / min, and the micropolymer capsules are injected into the sand filling pipe or core model.
[0049] The present invention can regulate the density of polymer capsules so that the scanned image of the polymer capsules in the three-dimensional core can be clearly segmented, and the position of the microcapsules can be accurately located in the core displacement scan, which is convenient for more accurate research on the migration law of the polymer capsules in the three-dimensional scanning experiment.
[0050] The beneficial effects of the present invention are:
[0051] (1) Using a high-viscoelastic polymer grafted with a high molecular weight monomer as the core material, the high-viscoelastic polymer can be released after the capsule ruptures to enhance the oil displacement effect. At the same time, the density difference between the polymer capsule and other phases is increased, thereby achieving precise positioning of the polymer capsule during the scanning process.
[0052] (2) Cellulose nanocrystal-alginate hydrogel is used as the polymer capsule wall material to enhance the elasticity of the polymer capsule shell and have slow release properties, thereby achieving a slow viscosity increase effect.
[0053] (3) Polymer capsules are generated by a microfluidic device, and the shell of the polymer capsules is cured by ultraviolet light to ultimately form stable polymer capsule solid particles with a core-shell structure.
[0054] (4) The prepared polymer capsules are injected into a sand-filled tube or an actual core, and a three-dimensional image of the sand-filled tube or the core is created using computed tomography. Through image processing, the microscopic seepage mechanisms of the polymer capsules in the actual formation environment, such as the migration and adsorption mechanism, deformation and plugging mechanism, and rupture and diffusion mechanism, are studied. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 A schematic diagram of the process of preparing polymer capsules using the microfluidic device of the present invention;
[0056] Figure 2 This is a schematic diagram of the structure of the test system of the present invention;
[0057] Figure 3 This is a structural schematic diagram of the wire take-up box of the present invention;
[0058] Figure 4 is a schematic diagram of the clamp of the present invention;
[0059] Figure 5 is a schematic diagram of the stage of the present invention;
[0060] Figure 6 It is a top view schematic diagram of the stage of the present invention;
[0061] Figure 7 Schematic diagram of core scanning slice after displacement of polymer capsules grafted with high molecular weight monomers;
[0062] Figure 8 This is a three-dimensional schematic diagram of polymer capsule core flooding;
[0063] Fig. 9 Schematic diagram of three-dimensional reconstruction of polymer capsule and crude oil distribution;
[0064] Fig.10 Schematic diagram of the three-dimensional reconstruction of the distribution of polymer capsules in pore throats;
[0065] Fig.11 The figure is a schematic diagram of the overall preparation and testing process of the polymer capsule of the present invention;
[0066] Figure 1 Middle: 30-micro displacement pump A, 31-micro displacement pump C, 32-micro syringe C, 33-micro syringe A, 34-catheter C, 35-catheter A, 36-co-flow and confocal combined capillary, 37-micro displacement pump B, 38-micro syringe B, 39-beaker, 40-polymer capsule, 41-ultraviolet lamp;
[0067] Figure 2-6Middle: 1-fluid injection and pressure control acquisition device, 2-temperature control box, 3-displacement pump, 4-X-ray source, 5-moving platform, 6-stage, 7-detector, 8-clamp, 9-CCD camera, 10-receiving box, 11-waste liquid tank, 12-pipeline, 13-spring, 14-winding reel, 15-fixed column, 16-CT scanning main console, 17-displacement outlet, 18-confining pressure outlet, 19-confining pressure inlet, 20-displacement inlet, 21-temperature sensor, 22-fixed head, 23-conversion table, 24-screw interface A, 25 screw interface B, 26-fixed pipe, 27-rubber sleeve, 28-core, 29-lead box;
[0068] Figure 7-8 Middle: From white to black, they are polymer capsules, rocks, and crude oil;
[0069] Fig. 9 In the middle, dark gray is the polymer capsule and light gray is the oil phase;
[0070] Fig.10 In the figure, the dark grey is the polymer capsule and the light grey is the rock. DETAILED DESCRIPTION
[0071] The present invention will be further described below by way of embodiments in conjunction with the accompanying drawings, but is not limited thereto.
[0072] like Figure 1-11 shown.
[0073] Embodiment 1:
[0074] A method for preparing a polymer capsule comprises the following steps:
[0075] (1) Measure the density of rock particles and the density of the displaced phase;
[0076] The density of rocks is measured using nuclear magnetic resonance technology. The density of conventional rocks is 2.2-2.8 g / cm 3 The density of the displaced phase is measured using a densitometer. The displaced phase is crude oil, and the density of conventional crude oil is 0.8-0.95 g / cm 3 The density of the polymer solution used is measured by a densitometer.
[0077] (2) Select appropriate original high-viscoelastic polymer and high molecular weight monomer, measure the density of the original polymer solution, and set the mixing ratio of the original polymer and the high molecular weight monomer according to the density difference between the original polymer solution and the rock particles and the displaced phase; synthesize the high-density target polymer grafted with the high molecular weight monomer as the core material through chemical grafting method;
[0078] The original polymer is one of polyacrylamide, polyvinylamide, sulfonated polyacrylic acid, sulfonated polyacrylamide, acrylic acid-sulfonated acrylic acid polymer, sulfonated polyvinyl alcohol, and sulfonated polyethylene;
[0079] The high molecular weight monomer is one of brominated phenol, isobutyl methacrylate and vinyl dimethoxy silane;
[0080] The method for preparing the target polymer comprises the following steps:
[0081] (2-1) According to the density difference between the original polymer solution and the rock particles and the displaced phase, the mixing ratio of the original polymer and the high molecular weight monomer is adjusted, and the ratio varies in the range of 1:1-1:10; the mass fraction of the polymer in the original polymer solution is 40-60%;
[0082] (2-2) adding 0.1%-2% of an inorganic catalyst according to the ratio, wherein the inorganic catalyst is one of hydrogen peroxide, ammonium persulfate, peracetic acid, and ethyl peroxyacetate. The higher the proportion of the high molecular weight monomer, the greater the amount of the inorganic catalyst added. The mass ratio of the original polymer, the high molecular weight monomer, and the inorganic catalyst is 1:0.1:0.05;
[0083] (2-3) The entire preparation was carried out under a nitrogen atmosphere at 80 °C and stirred at 500 r / min for 6 h.
[0084] (3) Preparation of polymer capsules by microfluidics;
[0085] The wall material of the polymer capsule was composed of cellulose nanocrystal-alginate hydrogel, which was dispersed at 500 r / min for 5 h, with a cellulose nanocrystal content of 0.15 wt% and an alginate content of 3%;
[0086] The cellulose nanocrystals have a length of 150 nm and a diameter of 13 nm, and the alginate is sodium alginate;
[0087] The polymer capsule is synthesized using a microfluidic device, which includes three microdisplacement systems and a co-flow and confocal combined capillary 36. The three microdisplacement systems are microdisplacement system A, microdisplacement system B, and microdisplacement system C. Each microdisplacement system includes a microdisplacement pump, a microinjector, and a catheter. Figure 1As shown, the micro displacement system A includes a micro displacement pump A 30, a micro syringe A 33, and a catheter A 35, the micro displacement system B includes a micro displacement pump B 37, a micro syringe B 38, and a catheter, and the micro displacement system C includes a micro displacement pump C 31, a micro syringe C 32, and a catheter C 34. An injection capillary and a collection capillary are provided in the co-flow and confocal combination capillary, and the injection capillary and the collection capillary both include a tapered body with a reduced inner diameter. The injection capillary and the collection capillary are arranged opposite to each other at their minimum openings, and a channel one is formed in the injection capillary, a channel two is formed between the collection capillary and the inner wall of the co-flow and confocal combination capillary, and a channel three is formed between the injection capillary and the inner wall of the co-flow and confocal combination capillary;
[0088] The preparation method comprises the following steps:
[0089] (3-1) The target polymer is loaded in the microdisplacement system A as the core material and injected from channel one; the cellulose nanocrystal-alginate hydrogel is loaded in the microdisplacement system B as the wall material and injected from channel two; the organic solution is loaded in the microdisplacement system C as the intermediate phase and injected from channel three; the organic solution is one of ethanol, isopropanol, undecanol, dodecanol, benzyl alcohol, octanol, ethylene glycol dimethyl ether, ethylene glycol methyl ether, acetone, methyl tert-butyl ketone, ethyl acetate, butanone, toluene, and xylene;
[0090] (3-2) adjusting the flow rate range of the target polymer and the wall material, wherein the injection flow rate of the target polymer varies in the range of 1-100 μL / min, and the injection flow rate of the wall material varies in the range of 100-1000 μL / min, to generate a stable emulsion polymer;
[0091] (3-3) placing the generated emulsion polymer in a solution containing a cross-linking agent for stabilization for 2-4 hours to form a hydrogel shell, wherein the cross-linking agent is one of aluminum sulfate, calcium chloride, calcium nitrate, ammonium chloride, ferric nitrate, and aluminum chloride;
[0092] (3-4) using a UV lamp 41 to emit UV light to cure the shell of the polymer capsule, thereby forming a stable polymer capsule 40 in the beaker 39;
[0093] (3-5) Wash the polymer capsules twice with distilled water and ethanol respectively;
[0094] (3-6) After being placed in an oven at 35 °C for 24 h, pure and dry polymer capsule particles were obtained.
[0095] (4) The prepared polymer capsules are formulated into a solution and injected into a core saturated with oil. A core slice image is obtained by CT scanning. The grayscale value ranges of the polymer capsules, rock particles and crude oil in the scanned image are determined by image processing software, such as dragonfly. If the grayscale value ranges of the polymer capsules, rock particles and crude oil overlap by more than 10%, the process returns to step (2) to adjust the mixing ratio of the original polymer and the high molecular weight monomer and to prepare the polymer capsules again.
[0096] The calculation formula of overlap is shown in formula (1):
[0097] (1)
[0098] in: d is the overlap between range 1 and range 2, %; a is the length of range 1; b is the length of range 2, c It is the length of the overlap between range 1 and range 2. Range 1 and range 2 refer to the grayscale value ranges for which the overlap needs to be calculated. For example, when calculating the overlap between the grayscale value ranges of polymer capsules and crude oil, range 1 is the grayscale value range of polymer capsules, and range 2 is the grayscale value range of crude oil; when calculating the overlap between the grayscale value ranges of polymer capsules and rocks, range 1 is the grayscale value range of polymer capsules, and range 2 is the grayscale value range of rocks.
[0099] For example, the grayscale value range of the polymer capsule is [150, 180], the grayscale value range of crude oil is [40, 100], and the grayscale value range of rock is [170, 255]. Then, the overlap between the grayscale value range of the polymer capsule and the crude oil is: , the gray value range overlap between the polymer capsule and the rock is: , if the overlap between the gray value range of the polymer capsule, the rock and the crude oil is less than 10%, then the polymer capsule meets the requirements.
[0100] The method of step (4) includes the following:
[0101] Step 1: Inject the prepared polymer capsule into the sand filling tube or actual rock core of the test system. Figure 2-6 As shown, it includes a displacement pump 3, a fluid injection and pressure control acquisition device 1, and a lead box 29. A stage 6 is provided in the lead box, and a clamp 8 is provided on the stage. The clamp can be a sand-filled tube clamp or a core clamp. An X-ray source 4, a CCD camera 9, and a detector 7 are provided around the clamp. The X-ray source is connected to a CT scanning main console 16 outside the lead box, the clamp is connected to the displacement pump 3 outside the lead box, and the fluid injection and pressure control acquisition device is connected to the displacement pump;
[0102] The test system is also provided with a temperature control box 2, which is connected to the displacement pump 3 and is used to control the temperature of the liquid in the displacement pump;
[0103] A conversion platform 23 is provided above the stage 6, and a moving platform 5 is provided below the stage. The moving platform is used to drive the upper device to move. The conversion platform is provided with screw interfaces, including three screw interfaces A 24 and one screw interface B 25. The clamp is connected to the conversion platform through the screw interfaces, which is convenient for fixing and replacement.
[0104] A wire take-up box 10 is provided in the lead box, and the wire take-up box includes a shell, a fixed column 15 is provided in the shell, a wire reel 14 is provided through the fixed column, and spring springs 13 are provided on the fixed columns at both ends of the wire reel. The pipeline 12 in the lead box is wound on the wire reel; the wire take-up box is used to collect the pipelines in the lead box neatly;
[0105] The clamp includes a fixed tube 26, in which a core 28 is arranged through a rubber sleeve 27, and a displacement inlet 20, a confining pressure inlet 19, a displacement outlet 17, and a confining pressure outlet 18 are respectively arranged at both ends of the fixed tube. A temperature sensor 21 is respectively arranged at both ends of the fixed tube. The bottom of the fixed tube is connected to the conversion platform through a fixed head 22, and one end of the fixed tube is connected to a waste liquid tank 11.
[0106] In this embodiment, if the seepage of the polymer capsule in the actual formation environment is to be studied, the sand-filled tube or the core is first vacuumed and saturated with simulated formation water to calculate the porosity and permeability of the sand-filled tube or the core model. The formulas for the permeability and porosity of the sand-filled tube or the core model are shown in equations (2) and (3):
[0107] (2)
[0108] in: k - Permeability of sand packs or core models, ; Q - In pressure difference Flow rate through sand-filled tube or core model, cm 3 / s; A - Cross-sectional area of sand filling tube or core model sand, cm 2 ; L - Length of sand filling tube or core model sand, cm; -Viscosity of the injected fluid, mPa·s; - Pressure difference before and after the fluid passes through the sand packing tube or core model, 10 5 Pa;
[0109] (3)
[0110] in: -Porosity of sand packs or core models; V孔 - Pore volume of sandfill or core model, obtained by weighing, cm 3 ; A - Cross-sectional area of sand filling tube or core model sand, cm 2 ; L - Length of sand filling tube or core model sand, cm;
[0111] Then, the micropolymer capsules are loaded into the displacement pump, the confining pressure fluid is injected, the confining pressure and its temperature are measured, and when the temperature detected by the temperature sensor reaches the formation temperature and the pressure in the fluid injection and pressure control acquisition device reaches the formation pressure range, the displacement pump is turned on, the flow rate is set to 1 μL / min, and the micropolymer capsules are injected into the sand filling pipe or core model.
[0112] Step 2: Use the CT Scan Console to create a sand fill tube or actual core slice.
[0113] Step 3: Filter and sharpen the scanned images, and segment the rock phase, pore phase, polymer capsule phase and pure water phase according to the grayscale values of different phases. Use 3D core reconstruction technology to construct a digital core. Since there is a large density difference between polymer capsules and rock, oil phase and pure water phase, the polymer capsule phase can be accurately analyzed. Combined with the 3D digital core, the state of polymer capsules between the core pores can be studied more three-dimensionally. By injecting different amounts of solution into the same core, the displacement channel inside the core is studied, the distribution of polymer capsules is located, and the migration law of polymer capsules is presented in 3D visualization. Then, the displacement of crude oil and the change in the distribution of polymer capsules at the same position are studied, and the oil displacement mechanism of polymer capsules is analyzed.
[0114] Figure 7 This is a schematic diagram of the core scanning slice after the displacement of the polymer capsule grafted with high molecular weight monomer. Figure 8 The three-dimensional schematic diagram of polymer capsule core flooding is shown in Figure 2. By performing operations such as sharpening and image segmentation on the scanned image, the following can be obtained: Fig. 9 The distribution of crude oil and polymer capsules inside the core is shown in Figure 2. Fig.10 Shown is the distribution of polymer capsules in the pore throats.
[0115] Example 2
[0116] A method for preparing a polymer capsule, wherein the steps are as described in Example 1, except that in step (2-2), the mass ratio of the original polymer, the high molecular weight monomer, and the inorganic catalyst is 1:0.02:0.002. In step (2-3), the mixture is stirred at 500 r / min at a temperature range of 65°C for 9 hours.
[0117] In step (3), the wall material of the polymer capsule is composed of cellulose nanocrystal-alginate hydrogel, which is dispersed at 500 r / min for 4 hours, with a cellulose nanocrystal content of 0.05 wt% and an alginate content of 1%. The cellulose nanocrystals have a length of 100 nm and a diameter of 3 nm, and the alginate is calcium galacturonate.
[0118] Example 3
[0119] A method for preparing a polymer capsule, wherein the steps are as described in Example 1, except that in step (2-2), the mass ratio of the original polymer, the high molecular weight monomer, and the inorganic catalyst is 1:0.2:0.1. In step (2-3), the mixture is stirred at 500 r / min for 4 h at a temperature range of 85°C.
[0120] In step (3), the wall material of the polymer capsule is composed of cellulose nanocrystal-alginate hydrogel, which is dispersed at 500 r / min for 6 h, with a cellulose nanocrystal content of 0.3 wt% and an alginate content of 6%. The cellulose nanocrystals have a length of 200 nm and a diameter of 20 nm, and the alginate is one of carrageenan and guar gum.
[0121] While embodiments of the present invention have been shown and described, it will be apparent to those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a polymer capsule, characterized in that: The steps include: (1) Measure the density of rock and displaced phase; (2) Selecting the original polymer and the high molecular weight monomer, measuring the density of the original polymer solution, and setting the mixing ratio of the original polymer and the high molecular weight monomer according to the density difference between the original polymer solution and the rock particles and the displaced phase; A high-density target polymer grafted with a high-molecular-weight monomer is synthesized as a core material by a chemical grafting method; the original polymer is one of polyacrylamide, polyvinylamide, sulfonated polyacrylamide, and sulfonated polyvinyl alcohol; the high-molecular-weight monomer is one of brominated phenol, isobutyl methacrylate, and vinyl dimethoxy silane; (3) Preparation of polymer capsules by microfluidics; The polymer capsule is synthesized using a microfluidic device, which includes three micro-displacement systems and a co-flow and confocal combination capillary. The three micro-displacement systems are respectively a micro-displacement system A, a micro-displacement system B, and a micro-displacement system C. Each micro-displacement system includes a micro-displacement pump, a micro-injector, and a catheter. An injection capillary and a collection capillary are provided in the co-flow and confocal combination capillary. The injection capillary and the collection capillary both include a cone. The minimum openings of the injection capillary and the collection capillary are arranged opposite to each other. Channel 1 is formed in the injection capillary, channel 2 is formed between the collection capillary and the inner wall of the co-flow and confocal combination capillary, and channel 3 is formed between the injection capillary and the inner wall of the co-flow and confocal combination capillary. The preparation method comprises the following steps: (3-1) The target polymer is contained in the micro-displacement system A as the core material and is injected from channel one; the cellulose nanocrystal-alginate hydrogel is contained in the micro-displacement system B as the wall material and is injected from channel two; the organic solution is contained in the micro-displacement system C as the intermediate phase and is injected from channel three, and the organic solution is one of ethanol, isopropanol, undecanol, dodecanol, benzyl alcohol, octanol, ethylene glycol dimethyl ether, ethylene glycol methyl ether, acetone, methyl tert-butyl ketone, ethyl acetate, butanone, toluene, and xylene; (3-2) adjusting the flow rate range of the target polymer and the cellulose nanocrystals, wherein the injection flow rate of the target polymer varies in the range of 1-100 μL / min, and the injection flow rate of the wall material varies in the range of 100-1000 μL / min, to generate a stable emulsion polymer; (3-3) placing the generated emulsion polymer in a solution containing a cross-linking agent for stabilization for 2-4 hours to form a hydrogel shell, wherein the cross-linking agent is one of aluminum sulfate, calcium chloride, calcium nitrate, ammonium chloride, ferric nitrate, and aluminum chloride; (3-4) curing the shell of the polymer capsule by ultraviolet light irradiation to form stable polymer capsule particles; (3-5) Wash the polymer capsules twice with distilled water and ethanol respectively; (3-6) Place in an oven at 35 °C for 24 h to obtain pure and dry polymer capsule particles; (4) The prepared polymer capsules are formulated into a solution and injected into a sand filling tube or an actual rock core of a test system, including the following steps: Step 1: Inject the prepared polymer capsule into the sand-filled tube or the actual core of the test system. The test system includes a displacement pump, a fluid injection and pressure control acquisition device, and a lead box. A stage is provided in the lead box. A clamp is provided on the stage. The clamp is a sand-filled tube type clamp or a core clamp. An X-ray source, a CCD camera, and a detector are provided around the clamp. The X-ray source is connected to the CT scanning main console outside the lead box. The clamp is connected to the displacement pump outside the lead box. The fluid injection and pressure control acquisition device is connected to the displacement pump. A temperature sensor is provided on the clamp. Step 2: Use the CT scanning console to create a sand-fill tube or actual core slice; Step 3: Filter and sharpen the scanned images, segment the rock phase, pore phase, polymer capsule phase and pure water phase according to the grayscale values of different phases, and construct a digital core through 3D core reconstruction technology; inject different amounts of solution into the same core to study the displacement channel inside the core, locate the distribution of polymer capsules, and present the migration law of polymer capsules in 3D visualization, thereby presenting the displacement of crude oil and the distribution change of polymer capsules at the same location; Determine the grayscale value ranges of the polymer capsules, rock particles and crude oil in the scanned image by using image processing software. If the grayscale value ranges of the polymer capsules, rock particles and crude oil overlap by more than 10%, return to step (2) to adjust the mixing ratio of the original polymer and the high molecular weight monomer, and prepare the polymer capsules again. The calculation formula of overlap is shown in formula (1): (1) in: d is the overlap between range 1 and range 2, %; a is the length of range 1; b is the length of range 2, c It is the length of the overlap between range 1 and range 2. Range 1 and range 2 respectively refer to the grayscale value ranges for which the overlap degree needs to be calculated.
2. The method for preparing a polymer capsule according to claim 1, characterized in that: In step (1), the rock density was measured using nuclear magnetic resonance technology and the rock density was between 2.2 and 2.8 g / cm 3 The density of the displaced phase is measured using a densitometer. The displaced phase is crude oil, which has a density of 0.8-0.95 g / cm 3 In step (2), the density of the polymer solution is measured by a densitometer.
3. The method for preparing a polymer capsule according to claim 1, characterized in that: In step (2), the method for preparing the target polymer comprises the following steps: (2-1) According to the density difference between the original polymer solution and the rock particles and the displaced phase, the mixing ratio of the original polymer and the high molecular weight monomer is adjusted, and the ratio varies in the range of 1:1 to 1:10; (2-2) Add 0.1%-2% of inorganic catalyst according to the ratio, the mass ratio of original polymer, high molecular weight monomer and inorganic catalyst is 1: (0.02-0.2): (0.002-0.1); (2-3) The entire preparation was carried out under a nitrogen atmosphere, at a temperature range of 65–85 °C and stirred at 500 r / min for 4–9 h.
4. The method for preparing a polymer capsule according to claim 3, characterized in that: In step (2-1), the mass fraction of the polymer in the original polymer solution is 40-60%; in step (2-2), the inorganic catalyst is one of hydrogen peroxide, ammonium persulfate, and peracetic acid.
5. The method for preparing a polymer capsule according to claim 1, characterized in that: In step (3), the wall material of the polymer capsule is composed of cellulose nanocrystal-alginate hydrogel, which is dispersed at 500 r / min for 4-6 h, and the cellulose nanocrystal content is in the range of 0.05wt%-0.3wt%, and the alginate content is in the range of 1%-6%; The length of the cellulose nanocrystal is 100-200nm, the diameter is 3-20nm, and the alginate is sodium alginate.
6. The method for preparing a polymer capsule according to claim 1, characterized in that: In step (4), the test system further includes one of the following solutions: a. The test system is also equipped with a temperature control box, which is connected to the displacement pump to control the temperature of the liquid in the displacement pump; b. A conversion platform is provided above the stage, a moving platform is provided below the stage, the conversion platform is provided with a screw interface, and the clamp is connected to the conversion platform through the screw interface; c. A wire take-up box is provided in the lead box, and the wire take-up box includes a shell, a fixed column is provided in the shell, a wire reel is provided through the fixed column, and a spring is provided on the fixed columns at both ends of the wire reel, and the pipeline in the lead box is wound on the wire reel; d. The clamp includes a fixed tube, the core is arranged in the fixed tube through a rubber sleeve, a displacement inlet, a confining pressure inlet, a displacement outlet, and a confining pressure outlet are respectively arranged at both ends of the fixed tube, a temperature sensor is respectively arranged at both ends of the fixed tube, and one end of the fixed tube is connected to a waste liquid tank.
7. The method for preparing a polymer capsule according to claim 1, characterized in that: In step (4), the sand-filled tube or core is first vacuumed and saturated with simulated formation water to calculate the porosity and permeability of the sand-filled tube or core model. The formulas for the permeability and porosity of the sand-filled tube or core model are shown in equations (2) and (3): (2) in: k - Permeability of sand packs or core models, ; Q - In pressure difference Flow rate through sand-filled tube or core model, cm 3 / s; A - Cross-sectional area of sand filling tube or core model sand, cm 2 ; L - Length of sand filling tube or core model sand, cm; -Viscosity of the injected fluid, mPa·s; - Pressure difference before and after the fluid passes through the sand packing tube or core model, 10 5 Pa; (3) in: -Porosity of sand packs or core models; V 孔 - Pore volume of sandfill or core model, obtained by weighing, cm 3 ; A - Cross-sectional area of sand filling tube or core model sand, cm 2 ; L - Length of sand filling tube or core model sand, cm; Then, the micropolymer capsules are loaded into the displacement pump, the confining pressure fluid is injected, the confining pressure and its temperature are measured, and when the temperature detected by the temperature sensor reaches the formation temperature and the pressure in the fluid injection and pressure control acquisition device reaches the formation pressure range, the displacement pump is turned on, the flow rate is set to 1 μL / min, and the micropolymer capsules are injected into the sand filling pipe or core.
Citation Information
Patent Citations
Hydrophobically modified sodium alginate material, and preparation method and application thereof
CN104098745A
Preparation method and application of slow-release antioxidant microcapsule
CN111418818A
Method for simulating oil recovery by using cellulose nanocrystals
CN112646560A
Method and system for improving recovery ratio by capsule polymer flooding
CN115853482A
Experimental device and monitoring method for measuring tackifying performance of capsule polymer
CN116429639A