Lithium supplement additive and preparation method and application thereof

By using a barrier layer with high reactive thermal stability in lithium-ion batteries to cover the nucleus, the problems of irreversible capacity loss and poor interface stability in lithium-ion batteries are solved, and higher battery capacity and charge and discharge are achieved Efficiency reduces side reactions and gas production.

CN117936781BActive Publication Date: 2024-11-15SHENZHEN DYNANONIC INNOVAZONE NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311664580.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-05
Publication Date
2024-11-15
Estimated Expiration
2043-12-05

AI Technical Summary

Technical Problem

During the first charging and discharging process of existing lithium-ion batteries, irreversible capacity loss caused by the formation of solid electrolyte interface film, which reduces the energy density and charging and discharging efficiency of the secondary battery. The stability of existing lithium-enriched materials is poor, especially in the air. The interface stability in the electrolyte is insufficient, resulting in side reactions and gas production problems.

Method used

A lithium supplement additive is used, which consists of a nuclear body and a barrier layer. The nuclear body contains the first lithium supplement material, and the barrier layer contains the second lithium supplement material. The thermal stability of the second lithium supplement material and carbon is higher than that of the second lithium supplement material. The thermal stability of the reaction between lithium-enriched materials and carbon is formed by sintering treatment to form a clad structure, improve the chemical and interface stability of the material, and further enhance the stability and capacity through the functional encapsulation layer.

Benefits of technology

It significantly improves the structural and interface stability of lithium supplement additives, reduces side reactions and gas production, enhances the capacity and charging and discharging efficiency of lithium-ion batteries, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117936781B_ABST
    Figure CN117936781B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of lithium-ion batteries, and in particular to lithium supplement additives and their preparation methods and applications. The lithium supplement additives include: a core body, containing a first lithium supplement material; a barrier layer, containing a second lithium supplement material, coating the core body; wherein the thermal stability of the reaction of the second lithium supplement material with carbon is higher than the thermal stability of the reaction of the first lithium supplement material with carbon. When the barrier layer is subjected to a carbon-containing thermal modification treatment, the barrier layer can effectively protect the core body, thereby improving the chemical stability of the first lithium supplement material in the core body, and at the same time can further improve the structure and interface stability of the lithium supplement additive, and can also play a role in enhancing the synergistic effect of composite lithium supplementation, thereby increasing the lithium supplement capacity. The steps of the preparation method include: in a protective atmosphere, mixing the second lithium supplement material and / or the precursor of the second lithium supplement material and the first lithium supplement material and then sintering them. The lithium supplement additive can be used in positive electrode material compositions and secondary batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to lithium supplement additives and preparation methods and applications thereof. Background Art

[0002] During the first charge and discharge process of lithium-ion batteries, a large amount of solid electrolyte interface film will be produced on the surface of the battery's negative electrode, consuming the limited lithium ions and electrolyte in the battery, causing irreversible capacity loss, reducing the energy density of the lithium-ion secondary battery and reducing the charge and discharge efficiency of the electrode material, limiting the application of lithium-ion batteries.

[0003] In the prior art, the first irreversible capacity loss of lithium batteries can be effectively compensated by adding lithium supplement materials to the positive electrode materials. For example, Li6CoO4 positive electrode lithium supplement material, Li6CoO4 has a high theoretical specific capacity (977mAh / g), low delithiation potential (3.4-3.6V), but like most lithium supplement materials, Li6CoO4 has poor stability in the air and poor interfacial stability in the electrolyte during charging and discharging, and interfacial side reactions can cause the electrolyte to decompose and produce gas. For this reason, materials such as carbon and metal oxides are generally used to coat lithium supplement materials. However, carbon will react with Li6CoO4 at high temperatures, causing the lithium supplement material to deteriorate. This problem also occurs in cobalt-based and nickel-based lithium supplement materials such as LiCoO2 and Li2NiO2, affecting the lithium supplement performance of the lithium supplement material. Summary of the invention

[0004] The purpose of the present application is to provide a lithium supplement additive and a preparation method thereof, aiming to solve the problem in the prior art that the lithium supplement material has poor stability and the coating treatment will affect the lithium supplement performance.

[0005] Another object of the present application is to provide a positive electrode material composition and a secondary battery, aiming to solve the problems of low capacity, low charge and discharge efficiency, and battery gas production of secondary batteries in the prior art.

[0006] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:

[0007] In a first aspect, the present application provides a lithium supplement additive, comprising:

[0008] A core body comprising a first lithium supplement material;

[0009] A barrier layer, comprising a second lithium supplement material, covering the core body;

[0010] The thermal stability of the reaction between the second lithium supplementing material and carbon is higher than the thermal stability of the reaction between the first lithium supplementing material and carbon.

[0011] The barrier layer in the lithium supplement additive of the present application can greatly improve the structural and interfacial stability of the lithium supplement additive, reduce the contact of the core with the external air, electrolyte, carbon materials, etc., and reduce interface side reactions. Moreover, the thermal stability of the reaction of the second lithium supplement material with carbon is higher than the thermal stability of the reaction of the first lithium supplement material with carbon. When the barrier layer is subjected to carbon-containing thermal modification, the barrier layer can effectively protect the core, thereby improving the chemical stability of the first lithium supplement material in the core, and at the same time can further improve the structural and interfacial stability of the lithium supplement additive. In addition, in addition to the first lithium supplement material contained in the core, the barrier layer also contains the second lithium supplement material, which can play a synergistic role in compounding lithium supplements and improve the lithium supplement capacity.

[0012] In a second aspect, the present application provides a method for preparing the lithium supplement additive of the present application, comprising the following steps:

[0013] In a protective atmosphere, the second lithium replenishing material and / or the precursor of the second lithium replenishing material and the first lithium replenishing material are mixed and then sintered.

[0014] The present application first mixes the second lithium supplement material and / or the precursor of the second lithium supplement material with the first lithium supplement material, so that the second lithium supplement material and / or the precursor of the second lithium supplement material are coated on the surface of the first lithium supplement material, and then performs a sintering treatment, so that the first lithium supplement material forms a core body, and the second lithium supplement material and / or the precursor generate the second lithium supplement material and further form a barrier layer, and the barrier layer coats the core body. Therefore, the lithium supplement additive of the present application can be prepared by this preparation method, and the structure and interface stability of the prepared lithium supplement additive are improved, and the preparation method process is controllable.

[0015] In a third aspect, the present application provides a positive electrode material composition, which contains the lithium supplement additive of the present application or the lithium supplement additive prepared by the preparation method of the present application.

[0016] The positive electrode material composition of the present application contains the lithium supplement additive of the present application, and the lithium supplement additive has good structure and interface stability, so the positive electrode material composition can reduce the side reaction with the electrolyte and reduce the gas generation phenomenon when used in the battery. In addition, the lithium supplement additive contained in the positive electrode material composition can replenish the lithium ions consumed in the first charge and discharge, thereby improving the capacity and charge and discharge efficiency.

[0017] In a fourth aspect, the present application provides a secondary battery, including a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet contains the positive electrode material composition of an embodiment of the present application.

[0018] The secondary battery of the present application contains the positive electrode material composition of the present application, so the side reaction between the positive electrode sheet and the electrolyte in the battery is small, and the gas generation phenomenon is reduced. In addition, the lithium supplement additive contained in the positive electrode sheet can supplement the lithium ions consumed in the first charge and discharge, thereby improving the capacity and charge and discharge efficiency of the secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0020] Figure 1 This is a schematic diagram of a lithium supplement additive according to an embodiment of the present application;

[0021] Figure 2 This is a schematic diagram of a lithium supplement additive according to an embodiment of the present application;

[0022] Figure 3 This is a TEM image of the lithium supplement additive of Example A1 of the present application;

[0023] Figure 4 This is the first charge and discharge curve of the lithium ion battery of Example B4 of the present application;

[0024] Reference numerals:

[0025] 1-core; 2-barrier layer; 3-functional encapsulation layer. DETAILED DESCRIPTION

[0026] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0027] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0028] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0029] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0030] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0031] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass in the embodiment description of the present application can be μg, mg, g, kg and other mass units known in the chemical industry.

[0032] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0033] In a first aspect, the present invention provides a lithium supplement additive as an embodiment of the present invention. The structure of the lithium supplement additive in the embodiment of the present invention is as follows: Figure 1 As shown, it includes a core body 1 and a barrier layer 2, and the barrier layer 2 covers the core body 1. The core body 1 contains a first lithium supplement material, and the barrier layer 2 contains a second lithium supplement material, and the thermal stability of the reaction between the second lithium supplement material and carbon is higher than that between the first lithium supplement material and carbon.

[0034] In the prior art, lithium supplement materials, especially high-capacity lithium supplement materials, often have poor interface stability and need to be provided with an encapsulation layer before they can be used. However, when the encapsulation layer is provided, especially when the carbon encapsulation layer is provided at high temperature, side reactions often occur with the lithium supplement material. Therefore, the lithium supplement additive in the embodiment of the present application includes a core 1 and a barrier layer 2 coating the core 1. Barrier means that the core 1 can be restricted from contacting the external environment, so that the barrier layer 2 is provided, which can greatly improve the structure and interface stability of the lithium supplement additive, reduce the contact of the core 1 with the external air, electrolyte, carbon materials, etc., and reduce interface side reactions. Moreover, the thermal stability of the reaction of the second lithium supplement material with carbon is higher than that of the first lithium supplement material with carbon. When the barrier layer 2 is subjected to a carbon-containing thermal modification treatment, the barrier layer 2 can effectively protect the core 1, thereby improving the chemical stability of the first lithium supplement material in the core 1, and at the same time can further improve the structure and interface stability of the lithium supplement additive. In addition, in addition to the first lithium supplement material contained in the core 1, the barrier layer 2 also contains a second lithium supplement material, which can play a role in compounding lithium supplementation and synergizing, thereby improving the lithium supplementation capacity.

[0035] About Nucleus 1:

[0036] The core 1 contains a first lithium supplement material, which can be a material with high lithium supplement capacity, but such materials often have poor stability, especially poor thermal stability in reaction with carbon. In some embodiments, the first lithium supplement material includes at least one of a cobalt-based lithium supplement material and a nickel-based lithium supplement material, and the general chemical formula is Li a M8O b , wherein M8 is Co and / or Ni, 1≤a≤6, 1≤b≤4. In the embodiment, at least one of Li6CoO4, LiCoO2, and Li2NiO2 may be included. The core first lithium supplement material mentioned above may be a primary particle or a secondary particle formed by the aggregation of primary particles, may be undoped or modified by doping, may be surface coated, pre-lithiated, etc. These cobalt-based and nickel-based lithium supplement materials have a high lithium supplement capacity, but these lithium oxides containing Ni or Co will react with carbon at high temperatures, such as being reduced by carbon, and it is difficult to directly use high-temperature carbon coating. By setting the barrier layer 2, the chemical stability of these first lithium supplement materials is effectively improved, thereby interacting with the isolation layer 2, and the stability and lithium supplement capacity can be compounded and enhanced. Li6CoO4 is optional, which has the advantages of high lithium supplement capacity and low delithiation potential, which is conducive to further improving the lithium supplement performance of the lithium supplement additive. In some embodiments, the first lithium replenishing material includes Li6CoO4, and the second lithium replenishing material includes Li5FeO4. The lithium replenishing additive obtained by the core 1 and the barrier layer 2 formed by these two materials has excellent structural and interface stability, high lithium replenishing capacity, rapid lithium desorption, and good lithium replenishing effect.

[0037] In some embodiments, the D50 particle size of the core body 1 is 0.5 to 5 μm. In the exemplary embodiment, it may include but is not limited to 0.5 μm, 1 μm, 3 μm, 5 μm and the range between any two values. The core body 1 with these particle sizes gives the lithium replenishing additive a higher lithium replenishing capacity, and is beneficial to the combination of the core body 1 and the barrier layer 2 to improve the structural and interface stability. In the embodiment, the ratio of the D90 particle size to the D50 particle size of the core body 1 can be 3:2 to 5:1; the ratio of the D50 particle size to the D10 particle size of the core body 1 can be 2:1 to 11:2, which can better control the particle size distribution of the core body 1, which is beneficial for the barrier layer 2 to better coat the core body 1 and exert a barrier effect.

[0038] When the lithium supplement additive of the present application also includes a functional encapsulation layer 3, in some embodiments, the mass content of the first lithium supplement material in the lithium supplement additive is 60% to 95%, and in the exemplary examples, it may include but is not limited to 60%, 70%, 80%, 90%, 95% and the range between any two values. The first lithium supplement material with these contents gives the lithium supplement additive a higher lithium supplement capacity, and is conducive to the combination of the core body 1 and the barrier layer 2 to improve the structural and interface stability.

[0039] About barrier layer 2:

[0040] In some embodiments, the second lithium supplement material includes Li5Fe 1-x1 M1 x1 O4、Li4Si 1-x2 M2 x2 O4、Li6Mn 1-x3 M3 x3 O4、Li8Zr 1-x4 M4 x4 O6、Li4Ti 1-x5 M5 x5 O4、Li8Sn 1-x6 M6 x6 O6、Li2Cu 1-x7 M7 x7 O2、Li x8 Z x9 At least one of, wherein M1, M2, M3, M4, M5, M6, and M7 are independently at least one of Fe, Si, Mn, Zr, Ti, Sn, and Cu, x1, x2, x3, x4, x5, x6, and x7 are independently 0 to 0.5, Z is at least one of S, O, N, P, and Se, 1≤x8≤3, and 1≤x9≤3. In the exemplary embodiment, the second lithium supplement material includes at least one of Li5FeO4, Li6MnO4, Li4SiO4, Li4TiO4, Li8ZrO6, Li8SnO6, Li2CuO2, Li2S, Li2O, Li3N, Li3P, and Li2Se. In the exemplary embodiment, Li5Fe 1-x1 M1x1 M1 in O4 can be different from the Fe element contained. In the example, Li4Si 1-x2 M2 x2 M2 in O4 can be different from the contained Si element, and so on. The second lithium supplement material of the barrier layer mentioned above can be undoped or modified by doping, and can be surface coated, pre-lithiation treated, etc. These second lithium supplement materials have high thermal stability in reaction with carbon, giving the barrier layer 2 a better barrier effect, improving the chemical stability of the first lithium supplement material in the core 1, and can further improve the structure and interface stability of the lithium supplement additive. These second lithium supplement materials also have a high lithium supplement capacity, which can further improve the lithium supplement effect of the lithium supplement additive. Li5FeO4 can be selected, which still has good thermal stability in reaction with carbon materials at 750°C. In addition to the excellent above-mentioned effects, Li5FeO4 also has good affinity with carbon materials. Therefore, carbon materials, especially vapor-deposited carbon, can be more firmly coated on the surface of Li5FeO4, that is, if there is also a carbon coating layer, the carbon coating layer and the barrier layer 2 can be tightly combined, which is beneficial to improve the structure and interface stability of the lithium supplement additive.

[0041] In some embodiments, the barrier layer 2 is a dense layer structure, and its coverage is 95% to 100%, and the through-hole rate is 0 to 5%. The dense layer structure is an effective way to achieve the barrier effect, which is conducive to improving the barrier effect of the barrier layer 2 and reducing or even avoiding the contact between the core 1 and the outside world. The coverage refers to the percentage of the area covered by the material of the barrier layer 2 on the surface of the core 1 to the total surface area of ​​the core 1. The ideal coverage is 100%.

[0042] In some embodiments, the D50 particle size of the second lithium supplement material is 20 to 100 nm. In the exemplary examples, it may include but is not limited to 20 nm, 40 nm, 60 nm, 80 nm, 100 nm and the range between any two values. The D50 particle size of these second lithium supplement materials is conducive to forming a dense layer structure to obtain a dense barrier layer 2. In the embodiment, the ratio of the D50 particle size of the core body 1 to the D50 particle size of the second lithium supplement material can be (10 to 200): 1. In the exemplary examples, it may include but is not limited to 10: 1, 50: 1, 100: 1, 200: 1 and the range between any two ratios. Such a particle size ratio is conducive to a larger particle size of the core body 1 and a smaller particle size of the second lithium supplement material. In this way, when the barrier layer 2 covers the core body 1, the proportion of through holes can be reduced, which is conducive to dense coating and improving the barrier effect. Among them, the smaller the particle size ratio, the more conducive to improving the density of the dense layer structure and improving the barrier effect of the barrier layer 2.

[0043] In some embodiments, the thickness of the barrier layer 2 is 40-200 nm, and in exemplary embodiments, it may include but is not limited to 40 nm, 80 nm, 120 nm, 200 nm, and any range between two values. The barrier layer 2 of these thicknesses is conducive to further improving the barrier effect and improving the structural and interface stability of the lithium supplement additive.

[0044] When the lithium supplement additive of the present application also includes a functional encapsulation layer 3, in some embodiments, the mass content of the second lithium supplement material in the lithium supplement additive is 3% to 40%. In the exemplary embodiment, it may include but is not limited to 3%, 8%, 13%, 20%, 30%, 40% and any range between two values. These contents of the second lithium supplement material are conducive to improving the barrier effect of the barrier layer 2.

[0045] About functional encapsulation layer 3:

[0046] In some embodiments, Figure 2 As shown, the lithium supplement additive further includes a functional encapsulation layer 3, which is coated on the surface of the barrier layer 2 away from the core 1. The functional encapsulation layer 3 can be an ion conductor encapsulation layer, an electronic conductor encapsulation layer, a hydrophobic encapsulation layer, etc., which have the corresponding effects of promoting the escape of lithium ions, improving conductivity, blocking external water, etc., and the encapsulation layer also has a barrier effect, which is beneficial to improving the structure and interface stability of the lithium supplement additive in the air and the electrolyte.

[0047] In some embodiments, the functional encapsulation layer 3 contains carbon materials, and the distribution morphology of the carbon materials is continuous and / or discontinuous. In the embodiments, the carbon materials include at least one of graphene, conductive carbon black, carbon nanotubes, carbon fibers, biomass carbon, amorphous carbon, and vapor-deposited carbon (e.g., CVD carbon). The functional encapsulation layer 3 containing carbon materials is beneficial to improving the electronic conductivity of the lithium supplement additive, and is beneficial to improving the lithium removal effect of the lithium supplement additive, especially the lithium removal effect at a high rate. Among them, CVD carbon coating is more conducive to the functional encapsulation layer 3 having a dense layer structure, further improving the barrier effect.

[0048] In some embodiments, the thickness of the functional encapsulation layer 3 is 10 to 100 nm, and in the exemplary examples, it may include but is not limited to 10 nm, 20 nm, 40 nm, 60 nm, 80 nm, 100 nm and the range between any two values. In some embodiments, the mass content of the functional encapsulation layer 3 in the lithium supplement additive is 1% to 10%, and in the exemplary examples, it may include but is not limited to 1%, 3%, 6%, 10% and the range between any two values. The functional encapsulation layer 3 of these thicknesses or mass contents is conducive to further improving the functionality of the encapsulation layer and improving the structural and interface stability.

[0049] For the lithium supplement additives in the embodiments of the present application, after testing:

[0050] In some embodiments, the water absorption rate of the lithium supplement additive at a humidity of 30% and a temperature of 25° C. is less than 0.1 ppm / s. In a demonstrative example, the water absorption rate may include but is not limited to 0.001 ppm / s, 0.005 ppm / s, 0.01 ppm / s, 0.05 ppm / s, 0.09 ppm / s and any range between two values, so that the lithium supplement additive has good hydrophobicity and good processing performance.

[0051] In some embodiments, the specific surface area of ​​the lithium supplement additive is 0.5 to 10 m 2 / g, in the exemplary embodiment, may include but is not limited to 0.5m 2 / g, 1m 2 / g, 5m 2 / g, 10m 2 / g and the range between any two values.

[0052] In some embodiments, the mass percentage of impurities contained in the lithium supplement additive is less than 1%. Impurity content less than 1% means that the barrier layer 2 has a good barrier effect, effectively blocking the contact between the core 1 and the external environment or the carbon material, and reducing the occurrence of impurities generated by side reactions. In addition, in the embodiments, because it is difficult to achieve high purity when preparing cobalt-based lithium supplement materials such as Li6CoO4 in the prior art, they often contain impurities such as Li2O and CoO, and nickel-based lithium supplement materials also have similar problems. The control of impurity content in the lithium supplement additive in the embodiments of the present application is also conducive to reducing the impact of these impurities on performance.

[0053] The second aspect of the embodiment of the present application provides a method for preparing the lithium supplement additive of the embodiment of the present application, comprising the following steps:

[0054] S10. In a protective atmosphere, the second lithium replenishing material and / or the precursor of the second lithium replenishing material and the first lithium replenishing material are mixed and then sintered.

[0055] In the embodiment of the present application, the second lithium supplement material and / or the precursor of the second lithium supplement material and the first lithium supplement material are first mixed, so that the second lithium supplement material and / or the precursor of the second lithium supplement material are coated on the surface of the first lithium supplement material, and then sintering is performed, so that the first lithium supplement material forms a core body 1, and the second lithium supplement material and / or the precursor generate the second lithium supplement material and further form a barrier layer 2, the barrier layer 2 covers the core body 1, and after the sintering treatment, the barrier layer 2 is tightly combined with the core body 1. Therefore, the lithium supplement additive of the embodiment of the present application can be prepared by the preparation method of this embodiment, the structure and interface stability of the prepared lithium supplement additive are improved, and the preparation method process is controllable.

[0056] In some embodiments, the particle size of the first lithium supplement material is 0.5-5 μm. In the embodiments, the first lithium supplement material can be sieved, and can be sieved through 400 mesh to 300 mesh, so that the core body 1 in the prepared lithium supplement additive has a corresponding particle size.

[0057] In some embodiments, the first lithium-supplementing material in step S10 can be a first lithium-supplementing material precursor prepared by a solid phase method, a liquid phase method, etc., and then sintered to obtain the first lithium-supplementing material. Taking the preparation of Li6CoO4 as an example, LiOH and CoO can be mixed in a molar ratio of 6.3:1. Since LiOH will volatilize, LiOH can be slightly excessive. The reactants are fully mixed by a mixer, and then placed in a tubular furnace, heated to 750°C, kept warm for 20 hours, crushed, and sieved through 300 mesh to obtain Li6CoO4, i.e., the first lithium-supplementing material. The above steps are all carried out in a protective atmosphere.

[0058] The second lithium-supplementing material in step S10 can be the finished product of the second lithium-supplementing material in the lithium-supplementing additive of the above-mentioned text application embodiment. In the exemplary embodiment, the second lithium-supplementing material includes Li5FeO4. The precursor of the second lithium-supplementing material can be provided according to the type of the second lithium-supplementing material. Taking the second lithium-supplementing material as Li5FeO4 as an example, in some embodiments, the second lithium-supplementing material includes Li5FeO4, and the precursor includes an iron source and a lithium source. The iron source may include Fe2O3 and / or Fe(OH)3. In some embodiments, the particle size of the iron source may be 20 to 200 nm. In the exemplary embodiment, it may include but is not limited to 20 nm, 50 nm, 100 nm, 150 nm, 200 nm and the range between any two values. The lithium source may include LiOH and / or Li2O. In some embodiments, the particle size of the lithium source may be 10 to 200 nm. In the exemplary embodiment, it may include but is not limited to 10 nm, 20 nm, 50 nm, 100 nm, 200 nm and the range between any two values. These iron sources and lithium sources can be sintered to produce Li5FeO4, and these particle sizes are conducive to controlling the particle size of the second lithium supplement material, improving the density of the barrier layer 2, and improving the barrier effect.

[0059] In step S10, the molar ratio of the first lithium supplement material, the iron source, and the lithium source can be (4-60):1:(10-12). In the exemplary embodiment, it can include but is not limited to 4:1:10, 20:1:10, 40:1:11, and 60:1:12. These molar ratios can control the mass ratio of the core body 1 and the barrier layer 2 in the obtained lithium supplement additive, and control the relationship between the particle size of the core body 1 and the thickness of the barrier layer 2.

[0060] In step S10, the second lithium replenishing material and / or the precursor of the second lithium replenishing material and the first lithium replenishing material can be mixed by using a high-speed mixer in a protective atmosphere. Due to the input of a large amount of mechanical energy in this mixing method, the surface of the first lithium replenishing material can form a certain interface bonding force with the second lithium replenishing material coated on the surface, or with the precursor coated on the surface, and the bonding is tight, which is conducive to obtaining a close bonding between the barrier layer 2 and the core body 1 in the lithium replenishing additive, improving the structural stability, and is conducive to the second lithium replenishing material forming a dense layer structure to achieve dense coating.

[0061] In some embodiments, the protective atmosphere for the sintering treatment can be nitrogen, argon or other atmospheres, and the temperature for the sintering treatment can be 650-750°C. In the exemplary embodiment, it can include but is not limited to 650°C, 680°C, 720°C, 750°C and any range between two values. The sintering treatment time can be 5-30 hours. On the one hand, these temperatures allow the precursor used to prepare the second lithium replenishing material to generate the second lithium replenishing material, and on the other hand, it is conducive to the close combination of the core body 1 obtained by the sintering treatment and the barrier layer 2. On the other hand, the second lithium replenishing material and carbon have good reaction thermal stability at these temperatures.

[0062] In some embodiments, after the sintering treatment, the step of encapsulating the surface of the cooled sintered product is also included. For example, an ion conductor encapsulation layer can be formed as the functional encapsulation layer 3 by atomic layer deposition of metal oxides. For example, a catalyst Fe, Ni, Cu and other metal elements can be introduced (for example, plated on the surface) on the surface of the sintered product, and then graphene, carbon nanotubes, carbon fibers and other materials can be grown in situ on the surface to form a carbon material layer, so that the in-situ grown carbon material can form a dense layer structure. For example, the sintered product can be fully mixed with a solid or liquid carbon source (such as glucose, PVP, etc.) and then heat treated at 750°C for 3 hours to form amorphous carbon from the carbon source to obtain a carbon material layer.

[0063] Taking the formation of a vapor-deposited carbon layer as an example, in some embodiments, the following steps are further included after the sintering process:

[0064] S20. Heat-treating the sintered product in a protective atmosphere containing a gaseous carbon source, so that the gaseous carbon source forms a dense vapor-deposited carbon layer on the surface of the sintered product.

[0065] The gaseous carbon source can be methane, ethylene, acetylene, etc. The heat treatment temperature can be 550-750°C. In the exemplary embodiment, it can include but is not limited to 550°C, 600°C, 700°C, 750°C and any range between two values. The gaseous carbon source is formed into vapor deposited carbon. A dense CVD carbon layer can be formed on the surface of the sintered product through a rotary CVD process as a functional encapsulation layer 3.

[0066] A third aspect of the embodiments of the present application provides a positive electrode material composition, which contains the lithium supplement additive of the embodiments of the present application or the lithium supplement additive prepared by the preparation method of the embodiments of the present application.

[0067] The positive electrode material composition of the embodiment of the present application contains the lithium supplement additive of the embodiment of the present application, and the lithium supplement additive has good structure and interface stability, so the positive electrode material composition can reduce the side reaction with the electrolyte and reduce the gas generation phenomenon when used in the battery. In addition, the lithium supplement additive contained in the positive electrode material composition can replenish the lithium ions consumed in the first charge and discharge, thereby improving the capacity and charge and discharge efficiency.

[0068] The positive electrode material composition can be used in a positive electrode sheet, which can be a conventional positive electrode sheet structure of a secondary battery, such as including a current collector and a positive electrode active layer bonded to the surface of the current collector, wherein the positive electrode active layer contains the positive electrode material composition.

[0069] In some embodiments, the mass content of the lithium supplement additive in the above-mentioned embodiment of the present application contained in the positive electrode active layer can be 0.1-20wt%; preferably, 0.1-8wt%. The positive electrode active layer includes, in addition to the lithium supplement additive, a positive electrode active material, a binder and a conductive agent, wherein the binder can be a commonly used positive electrode binder, such as polyvinylidene chloride, soluble polytetrafluoroethylene, styrene-butadiene rubber, hydroxypropyl methylcellulose, methylcellulose, carboxymethyl cellulose, polyvinyl alcohol, acrylonitrile copolymer, sodium alginate, chitosan and chitosan derivatives. In the embodiment of the present application, the conductive agent can be a commonly used conductive agent, such as one or more of graphite, carbon black, acetylene black, graphene, carbon fiber, C60 and carbon nanotubes. The positive electrode active material includes one or more of lithium cobaltate, lithium manganate, lithium iron phosphate, lithium vanadium phosphate, lithium vanadium oxyphosphate, lithium fluorinated vanadium phosphate, lithium titanate, lithium nickel cobalt manganate, and lithium nickel cobalt aluminum.

[0070] In some embodiments, the positive electrode sheet preparation process can be: mixing the positive electrode active material, lithium supplement additive, conductive agent and binder to obtain positive electrode slurry, coating the positive electrode slurry on the current collector, and preparing the positive electrode sheet through drying, rolling, die cutting and other steps.

[0071] A fourth aspect of an embodiment of the present application provides a secondary battery, including a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet contains the positive electrode material composition of an embodiment of the present application.

[0072] The secondary battery of the present application embodiment includes necessary components such as a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, and of course other necessary or auxiliary components. Among them, the positive electrode sheet contains the positive electrode material composition of the above-mentioned application embodiment, that is, the positive electrode active layer contained in the positive electrode sheet contains the lithium supplement additive of the above-mentioned application embodiment.

[0073] The secondary battery of the embodiment of the present application contains the positive electrode material composition of the embodiment of the present application, so the side reaction between the positive electrode sheet and the electrolyte in the battery is small, and the gas generation phenomenon is reduced. In addition, the lithium supplement additive contained in the positive electrode sheet can supplement the lithium ions consumed in the first charge and discharge, thereby improving the capacity and charge and discharge efficiency of the secondary battery.

[0074] The following describes the invention in conjunction with specific embodiments.

[0075] Example A1

[0076] This embodiment provides a lithium replenishing additive and a preparation method thereof. The lithium replenishing additive includes a core body, a barrier layer, and a functional encapsulation layer. The core body is a first lithium replenishing material, which is Li6CoO4, and the barrier layer is a second lithium replenishing material, which is Li5FeO4, coating the core body. The functional encapsulation layer is a CVD carbon layer, which is coated on the surface of the barrier layer away from the core body.

[0077] The preparation method of the lithium supplement additive comprises the following steps:

[0078] S1: Preparation of the first lithium supplement material

[0079] LiOH and CoO were mixed in a molar ratio of 6.3:1, and the reactants were fully mixed by a mixer, and then placed in a tube furnace, heated to 750°C, kept warm for 20 hours, crushed, and sieved with a 300-mesh sieve to obtain Li6CoO4 with a D50 particle size of 1 μm, i.e., the first lithium supplement material. The above steps were all carried out in a protective atmosphere.

[0080] S2: Forming a barrier layer

[0081] The first lithium supplement material obtained in step S1, Fe2O3 (iron source, D50 particle size of 50nm), and LiOH (lithium source, D50 particle size of 80nm) are mixed with a high-speed mixer at a molar ratio of 30:1:11, and after mixing evenly, they are heated to 700°C for sintering and kept warm for 20 hours; the iron source and the lithium source form Li5FeO4 (the second lithium supplement material), which is a dense barrier layer, the first lithium supplement material forms a core body, and the barrier layer covers the core body; after cooling, pass through a 300-mesh sieve, and the above steps are all carried out in a protective atmosphere.

[0082] S3: Forming functional encapsulation layer

[0083] The product of step S2 is placed in a rotary furnace, rotated at a speed of 5 r / min, with acetylene as the gaseous carbon source and argon as the carrier gas at a flow rate of 200 sccm, and heat treated at 600°C for 2 hours to form CVD carbon (vapor deposited carbon) from acetylene. Through the above rotary CVD process, a dense CVD carbon layer is formed on the outer surface of the barrier layer as a functional encapsulation layer. The above steps are all carried out in a protective atmosphere.

[0084] Example A2

[0085] This embodiment provides a lithium replenishing additive and a preparation method thereof. The preparation method is different from that of Embodiment A1 only in that the second lithium replenishing material is changed to Li6MnO4, and the first lithium replenishing material, Fe2O3, and LiOH in a molar ratio of 30:1:11 in step S2 are changed to the first lithium replenishing material, MnO, and LiOH in a molar ratio of 15:1:11, and the rest remain unchanged.

[0086] Example A3

[0087] This embodiment provides a lithium supplement additive and a preparation method thereof. The preparation method is different from that of Embodiment A1 only in that the molar ratio in step S2 is changed from 30:1:11 to 60:1:11, and the rest remains unchanged.

[0088] Example A4

[0089] This embodiment provides a lithium supplement additive and a preparation method thereof. The preparation method is different from that of Embodiment A1 only in that the molar ratio in step S2 is changed from 30:1:11 to 4:1:11, and the rest remains unchanged.

[0090] Example A5

[0091] This embodiment provides a lithium supplement additive and a preparation method thereof. The preparation method is different from that of Embodiment A1 only in that the particle size of the iron source in step S2 is changed from 50 nm to 20 nm, and the particle size of the lithium source is changed from 80 nm to 10 nm, and the rest remains unchanged.

[0092] Example A6

[0093] This embodiment provides a lithium supplement additive and a preparation method thereof. The preparation method is different from that of Embodiment A1 only in that the particle size of the iron source in step S2 is changed from 50 nm to 100 nm, and the particle size of the lithium source is changed from 80 nm to 100 nm, and the rest remains unchanged.

[0094] Example A7

[0095] This embodiment provides a lithium supplement additive and a preparation method thereof. The preparation method is different from that of Embodiment A1 only in that the particle size of the iron source in step S2 is changed from 50 nm to 200 nm, and the particle size of the lithium source is changed from 80 nm to 200 nm, and the rest remains unchanged.

[0096] Example A8

[0097] This embodiment provides a lithium supplement additive and a preparation method thereof. The preparation method is different from that of Embodiment A1 only in that step S1 is changed to prepare Li2NiO2 as the first lithium supplement material, LiOH and CoO are changed to LiOH and NiO, the molar ratio is changed to 2.1:1, and the others remain unchanged.

[0098] Comparative Example A1

[0099] This comparative example provides a lithium supplementing additive and a preparation method thereof. The preparation method is different from that of Example A1 only in that: no barrier layer is included, step S2 is not included, and the first lithium supplementing material is directly subjected to step S3, and other aspects remain unchanged.

[0100] Comparative Example A2

[0101] This comparative example provides a lithium supplement additive and a preparation method thereof. The preparation method differs from Example A1 only in that: the barrier layer is changed to an Al2O3 coating layer, and step S2 is changed to "mixing the first lithium supplement material obtained in step S1 and Al2O3 particles with a D50 particle size of 100 nm in a high-speed mixer at a molar ratio of 30:1, and after mixing evenly, heating to 400°C for sintering to obtain Al2O3-coated Li6CoO4", and the rest remains unchanged.

[0102] Lithium-ion battery example:

[0103] The lithium supplement additives provided in the above-mentioned embodiments A1 to A8 and comparative examples A1 and A2 are respectively assembled into positive electrode sheets according to the following methods, and the positive electrode sheets are sequentially assembled into corresponding lithium ion battery embodiments B1 to B8 and comparative examples B1 and B2:

[0104] Positive electrode sheet: a lithium supplementing additive, SP and PVDF are mixed and homogenized in a mass ratio of 90:4:6 to prepare a positive electrode slurry, the positive electrode slurry is coated on the surface of an aluminum foil, vacuum dried overnight at 110°C, and rolled to obtain a positive electrode sheet; wherein the lithium supplementing additives are respectively those of the above Examples A1 to A8 and Comparative Examples A1 and A2, specifically, the positive electrode sheet of the lithium ion battery in Example B1 contains the lithium supplementing additive of Example A1, the positive electrode sheet of the lithium ion battery in Example B2 contains the lithium supplementing additive of Example A2, and so on, the positive electrode sheet of the lithium ion battery in Example B8 contains the lithium supplementing additive of Example A8, the positive electrode sheet of the lithium ion battery in Comparative Example B1 contains the lithium supplementing additive of Comparative Example A1; the positive electrode sheet of the lithium ion battery in Comparative Example B2 contains the lithium supplementing additive of Comparative Example A2;

[0105] Negative electrode: lithium sheet is used as negative electrode;

[0106] Electrolyte: Ethylene carbonate and ethyl methyl carbonate were mixed in a volume ratio of 3:7, and LiPF6 was added to form an electrolyte, and the concentration of LiPF6 was 1 mol / L;

[0107] Diaphragm: polypropylene microporous diaphragm;

[0108] Lithium-ion battery assembly: Assemble button-type lithium-ion full batteries in an inert atmosphere glove box in the order of lithium sheet-diaphragm-electrolyte-positive electrode sheet.

[0109] Related performance tests and result analysis

[0110] 1. Related tests of lithium supplement additives

[0111] 1.1 Water absorption rate test

[0112] The lithium supplement additives provided in the above Examples A1 to A8 and Comparative Examples A1 and A2 were placed in a constant temperature and humidity environment with a humidity of 30% and a temperature of 25° C. for 30 minutes, and the water absorption rate was tested by observing and comparing the mass change rate of the lithium supplement additives. The results are shown in Table 1;

[0113] 1.2 Impurity content test

[0114] The lithium supplement additives provided in the above-mentioned Examples A1 to A8 and Comparative Examples A1 and A2 were subjected to X-ray diffraction (XRD) test, and the test results were refined to analyze the content of impurities (the impurities here do not include the main components corresponding to the barrier layer and the encapsulation layer, but mainly refer to the unreacted reactants when synthesizing the core body and the barrier layer materials or the impurities caused by the reaction of carbon with the core body material). The results are shown in Table 1;

[0115] 1.3 Barrier layer and functional encapsulation layer thickness test

[0116] The lithium supplement additives provided in the above-mentioned Examples A1 to A8 and Comparative Examples A1 and A2 were characterized by a transmission electron microscope (TEM) to observe and test the thickness of the barrier layer and the encapsulation layer. The results are shown in Table 1. The TEM image of the lithium supplement additive in Example A1 is shown in Figure 3 As shown, Figure 3 There are also two dotted lines for identification, the bottom is the amorphous carbon encapsulation layer, the barrier layer is between the two dotted lines, and the top is the core body.

[0117] Table 1

[0118]

[0119] As can be seen from Table 1, the water absorption rates of Examples A1 to A8 are all below 0.1ppm / s, and the impurity contents are all below 1%, indicating that the designed double-layer coating can not only achieve the stability of the lithium supplement additive in the air (almost no water absorption), but also achieve the goal of not introducing new impurities. The impurity content of Comparative Example A1 is as high as 8.64%, and its water absorption rate is one order of magnitude higher than that of Examples A1 to A8. This is because there is no barrier layer in Comparative Example A1, resulting in the reaction of carbon and Li6CoO4 at high temperature after carbon coating, producing more impurities, such as Co element, etc., and due to the consumption of carbon, the carbon coating layer is not dense enough and has some holes, which inevitably causes an increase in water absorption. Comparative Example A2 uses an Al2O3 barrier layer, and the corresponding water absorption rate and impurity content are both low, indicating that Al2O3 is also a very good barrier layer, but since Al2O3 does not contain active lithium, it will reduce the overall gram capacity of the lithium supplement additive.

[0120] In addition, the thickness of the barrier layer and the particle size of the barrier layer raw material also have a certain influence on the final impurity content. Comparing Examples A1, A3, and A4, it can be seen that the thicker the barrier layer, the lower the corresponding impurity content. This may be because the thicker the barrier layer, the more difficult the contact between carbon and Li6CoO4, and the two will hardly react to produce impurities. Comparing Examples A5 to A7, it can be found that the smaller the particle size of the barrier layer raw material, the lower the corresponding impurity content. Similarly, the smaller the particle size of the barrier layer raw material, the denser the synthesized barrier layer product, and the better the barrier effect.

[0121] 2. Lithium-ion battery performance test:

[0122] The electrochemical performance of the lithium ion batteries of Examples B1 to B8 and Comparative Examples B1 and B2 was tested under the following test conditions:

[0123] High temperature storage gas production test method and conditions: At 60°C, each lithium ion battery assembled in the above lithium ion battery embodiment is fully charged at a rate of 0.055C and stored for 72 hours. A battery gas production test device is used to detect the gas production of the battery after the storage.

[0124] After the battery formation is completed, the lithium-ion battery is subjected to electrochemical performance test at room temperature of 25°C. The test conditions are as follows:

[0125] Constant current and constant voltage charging, the first cycle charging and discharging voltage is 2.5~4.3V, the current is 0.1C, and the cut-off current is 0.01C.

[0126] Among them, the first charge and discharge curve of Example B4 is as follows Figure 4 The test results of each case are shown in Table 2 below:

[0127] Table 2

[0128]

[0129]

[0130] It can be seen from Table 2 that the total storage gas production of Examples B1 to B7 is lower than 3mL / g, and the corresponding first charge gram capacity is higher than 750mAh / g. In addition to the low gram capacity (because the gram capacity of the Li2NiO2 core itself is relatively low), the total storage gas production of Example B8 is also low. The above results show that the double-layer coating structure can simultaneously achieve a higher first charge gram capacity and a lower total high-temperature storage gas production. High-temperature storage gas production mainly comes from the decomposition of the electrolyte. Since Examples A1 to A8 all have good interface coating, the side reaction of the lithium supplement additive with the electrolyte during the charging process is suppressed, and the corresponding total gas production is relatively small.

[0131] In Comparative Example B1, the high-temperature storage gas production exceeds 9mL / g, which is more than 2 times higher than that of Example B1, and the corresponding gram capacity is less than 600mAh / g. This is because carbon and Li6CoO4 undergo a chemical reaction at high temperature, the coating layer is damaged and not dense enough, resulting in serious gas production. At the same time, the core material of the lithium supplement additive is also consumed, resulting in a decrease in gram capacity. In Comparative Example B2, although the storage gas production is low, less than 3mL / g, the Al2O3 barrier layer does not provide any active lithium, and its electronic conductivity and ionic conductivity are low, which to a certain extent hinders the migration and release of active lithium in the core material Li6CoO4, increases impedance and polarization, and results in a low capacity (less than 400mAh / g).

[0132] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A lithium supplement additive, characterized in that: include: A core body comprising a first lithium supplement material; A barrier layer, comprising a second lithium supplement material, covering the core; Wherein, the thermal stability of the reaction between the second lithium supplement material and carbon is higher than the thermal stability of the reaction between the first lithium supplement material and carbon; The first lithium supplement material includes Li a M8O b , wherein M8 is Co or Ni, 1≤a≤6, 1≤b≤4; The second lithium supplement material includes Li5Fe 1-x1 M1 x1 O4、Li4Si 1-x2 M2 x2 O4、Li6Mn 1-x3 M3 x3 O4、Li8Zr 1-x4 M4 x4 O6、Li4Ti 1-x5 M5 x5 O4、Li8Sn 1-x6 M6 x6 O6、Li2Cu 1-x7 M7 x7 O2、Li x8 Z x9 At least one of the following, wherein M1, M2, M3, M4, M5, M6, and M7 are independently any one of Fe, Si, Mn, Zr, Ti, Sn, and Cu, x1, x2, x3, x4, x5, x6, and x7 are independently 0 to 0.5, Z is any one of S, O, N, P, and Se, 1≤x8≤3, and 1≤x9≤3.

2. The lithium supplement additive according to claim 1, characterized in that: The D50 particle size of the second lithium supplementing material is 20 to 100 nm; and / or The barrier layer is a dense layer structure, and its coverage is 95% to 100%, and its through-hole rate is 0 to 5%; and / or The thickness of the barrier layer is 40-200 nm.

3. The lithium supplement additive according to claim 1 or 2, characterized in that: The D50 particle size of the core body is 0.5 to 5 μm; and / or The ratio of the D90 particle size to the D50 particle size of the core body is 3:2 to 5:1; and / or The ratio of the D50 particle size to the D10 particle size of the core body is 2:1 to 11:2; and / or The ratio of the D50 particle size of the core body to the D50 particle size of the second lithium supplementing material is 10:1 to 200:

1.

4. The lithium supplement additive according to claim 1 or 2, characterized in that: The first lithium supplement material includes Li6CoO4, and the second lithium supplement material includes Li5FeO4; and / or The lithium supplement additive further includes a functional encapsulation layer, which is coated on a surface of the barrier layer away from the core body.

5. The lithium supplement additive according to claim 4, characterized in that: The functional encapsulation layer contains a carbon material, wherein The distribution morphology of the carbon material is continuous and / or discontinuous; and / or The carbon material includes at least one of graphene, conductive carbon black, carbon nanotubes, carbon fibers, biomass carbon, amorphous carbon, and vapor deposited carbon; and / or The thickness of the functional encapsulation layer is 10 to 100 nm; and / or The mass content of the functional encapsulation layer in the lithium supplement additive is 1% to 10%; and / or The mass content of the second lithium supplement material in the lithium supplement additive is 3% to 40%; and / or The mass content of the first lithium supplement material in the lithium supplement additive is 60% to 95%.

6. The lithium supplement additive according to any one of claims 1, 2 and 5, characterized in that: The water absorption rate of the lithium supplement additive at a humidity of 30% and a temperature of 25° C. is less than 0.1 ppm / s; and / or The specific surface area of ​​the lithium supplement additive is 0.5 to 10 m 2 / g; and / or The mass percentage of impurities contained in the lithium supplement additive is less than 1%.

7. A method for preparing the lithium supplement additive according to any one of claims 1 to 6, characterized in that: The steps include: In a protective atmosphere, the second lithium supplement material and / or the precursor of the second lithium supplement material and the first lithium supplement material are mixed and then sintered.

8. The preparation method according to claim 7, characterized in that: The sintering temperature is 650-750°C; and / or The particle size of the first lithium supplementing material is 0.5 to 5 μm; and / or The second lithium supplement material includes Li5FeO4; and / or The precursor includes an iron source and a lithium source.

9. The preparation method according to claim 8, characterized in that: The particle size of the iron source is 20 to 200 nm; and / or The particle size of the lithium source is 10 to 200 nm.

10. The preparation method according to any one of claims 7 to 9, characterized in that: After the sintering process, the following steps are also included: The sintered product is heat treated in a protective atmosphere containing a gaseous carbon source, so that the gaseous carbon source forms a dense vapor-deposited carbon layer on the surface of the sintered product.

11. A positive electrode material composition, characterized in that: The positive electrode material composition contains the lithium supplement additive according to any one of claims 1 to 6 or the lithium supplement additive prepared by the preparation method according to any one of claims 7 to 10.

12. A secondary battery, comprising a positive electrode sheet and a negative electrode sheet, characterized in that: The positive electrode sheet contains the positive electrode material composition according to claim 11.