A method for remanufacturing a hob cutter ring by vibration-assisted laser cladding
Through the use of mechanical vibration-assisted laser cladding and gradient materials, the cracks and stress imbalance caused by excessive heat input in the remanufacturing of the shield machine hob ring is solved, and the improvement of the blade ring performance and effective utilization of resources is achieved. , reducing construction costs.
Patent Information
- Application Number
- CN202311793299.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-25
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-12-25
AI Technical Summary
In the prior art, when remanufacturing the hob ring of the shield machine, excessive heat input leads to cracks and stress imbalance, resulting in reduced performance of the blade ring and serious waste of resources. Remanufacturing technology needs to be improved to improve performance and utilization.
The mechanical vibration-assisted laser cladding method is adopted, and the cladding is carried out using gradient materials, and the residual stress is reduced by vibration aging, grains are refined, the element distribution is uniform, and the cladding and vibration treatment are repeated until the original size is restored.
It effectively reduces cracks and stress, improves the performance of the knife ring, and makes its performance no less than that of new products, saves construction costs, extends the service life of the knife ring, and reduces resource waste.
Smart Images

Figure CN117943553B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tunnel boring tools, and in particular relates to a method for remanufacturing a hob cutter ring through vibration-assisted laser cladding. Background Art
[0002] The shield machine is a tunnel boring machine that uses the shield method. It is the core equipment in infrastructure and a symbol of a country's underground construction equipment manufacturing level. The shield cutter ring is a key part for the shield machine to perform rock breaking tasks. It is often in extreme service conditions of huge extrusion, bending, torsion, impact, wear and local high temperature. Therefore, after a period of use, it will fail due to normal wear, eccentric wear, fracture, peeling, deformation, etc. According to statistics, the cost of tool consumption in shield machine construction accounts for about 1 / 5 to 1 / 4 of the project cost, and it is as high as about 1 / 3 when the geological conditions are bad; the time consumed by tool replacement accounts for about 1 / 3 of the project construction time. At the same time, the cutter rings that are removed cannot be reused, resulting in a waste of resources and an increase in excavation costs. However, the failure form of most cutter rings is normal wear, and most of the structures are still intact. Therefore, it is of great significance and value to remanufacture the failed cutter rings.
[0003] Since the mechanical properties and integrity of the cutter ring decrease after serving under extreme working conditions, during the remanufacturing process of the cutter ring, excessive stress should be avoided and structures that cause unbalanced stress distribution should be avoided to avoid secondary damage to the cutter ring. Only under this premise can the cutter ring be strengthened to maintain or even exceed the original performance.
[0004] At present, the main method of remanufacturing failed cutter rings is cladding, but the heat input of cladding is large, which can easily lead to cracks in the cutter ring and cause cracking and peeling of the additive manufacturing coating. It also has the disadvantages of long cladding time and excessive heat input, which causes coarse grains and reduces performance. Compared with cladding, laser cladding has a small heat input, but its rapid melting and solidification process can also cause cracks.
[0005] Therefore, it is urgent to improve the remanufacturing technology of failed cutter rings, eliminate cracks in the laser cladding process, and reduce the residual stress that causes crack initiation to ensure the performance of the workpiece. Mechanical vibration-assisted laser cladding has been proven to be an effective method to reduce temperature gradients and thus residual stress, break dendrites to refine grains, interrupt intercrystalline bridges to allow liquid to shrink in time to prevent small cracks from forming inside the metal, and promote uniform distribution of elements. Vibration aging can effectively reduce residual stress and has been widely used in the post-processing of welded parts. In addition, gradient materials can achieve a smooth transition of materials and stresses, avoiding cracking caused by excessive differences in material properties. The present invention uses mechanical vibration-assisted laser cladding to clad gradient materials on the surface of the cutter ring, and combines vibration aging to reduce residual stress, to develop a remanufactured cutter ring with performance no less than that of a new cutter ring, so as to improve the utilization rate of the cutter ring, save construction costs, and expand the remanufacturing path of the cutter ring. Summary of the invention
[0006] The object of the present invention is to provide a method for remanufacturing a hob cutter ring by vibration-assisted laser cladding to solve the problems raised in the above-mentioned background technology.
[0007] To achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for remanufacturing a hob cutter ring by vibration-assisted laser cladding comprises the following steps:
[0009] 1) Remove the failed cutter ring from the hob, flatten it and measure its shape and size;
[0010] 2) Mechanical vibration-assisted laser cladding was used to repair the cutter ring, with 2 layers of cladding;
[0011] 3) Vibration aging treatment after cladding 2 layers;
[0012] 4) Repeat steps 2) and 3) until the knife circle is restored to its original size.
[0013] Further, in step 2), laser cladding is performed using a gradient material, and the cladding material is a Ni-based powder and a Fe-based powder with a size of 53 μm to 154 μm;
[0014] Among them, the first to fourth layers are clad with Ni-based powder;
[0015] From the 5th to the 10th layer, 80% Ni-based powder + 20% Fe-based powder is used for cladding;
[0016] From the 11th to the 15th layer, 50% Ni-based powder + 50% Fe-based powder are used for cladding;
[0017] From the 16th to the 20th layer, 20% Ni-based powder + 80% Fe-based powder is used for cladding;
[0018] The remaining layers are all clad with Fe-based powder.
[0019] Furthermore, the thickness of the 1st to 4th layers is 2 mm; the thickness of the 5th to 10th layers is 2.6 mm; the thickness of the 11th to 15th layers is 2.6 mm; the thickness of the 16th to 20th layers is 2.6 mm; the total thickness of the cladding layer is 25 to 30 mm.
[0020] Furthermore, the powder feeding method of laser cladding is coaxial powder feeding, the laser power range is 1400W, the scanning speed range is 10mm / s, the powder feeding amount is 10~15g / min, the overlap rate is 60%, and the laser beam is a circular spot with a diameter of 3.0mm.
[0021] Furthermore, the mechanical vibration is characterized by a one-dimensional mechanical vibration in a direction perpendicular to the laser irradiation direction, with a vibration frequency of 116.7 Hz and a vibration amplitude of 18 μm.
[0022] Furthermore, the frequency of the vibration aging treatment is taken as any value in the sub-resonance zone of the workpiece, and the corresponding acceleration is 71.6m / s 2 , the vibration aging treatment time is 30min.
[0023] Furthermore, the mechanical vibration and the vibration aging are vibrated by a vibration table, and the vibration table comprises:
[0024] An inverted pair of rails, each end of which is fixedly connected;
[0025] The exciter is installed at one end of the rail and is rigidly connected to the rail;
[0026] The tool fixture is installed in the middle of the rail and is rigidly connected to the rail. The tool fixture is used to rigidly clamp the tool ring;
[0027] Vibration detector, used to be attached to the side of the knife ring;
[0028] Two pairs of seismic isolation rubber pads are placed at a distance of 2 / 9 of the length of the rails at both ends of the rails.
[0029] Furthermore, in step 1), a flattening process is performed and the shape and size are measured, including:
[0030] Grind the part of the surface of the used knife ring to be repaired, and then clean the surface of the knife ring;
[0031] The shape and size of the waste cutter ring are measured with a measurement accuracy of 0.001mm to determine the size of the cutter ring to be restored. Beneficial Effects
[0032] The present invention provides a method for remanufacturing a hob cutter ring by vibration-assisted laser cladding, which uses a laser cladding technology with low heat input and good formability for remanufacturing, and introduces mechanical vibration during the laser cladding process, which can reduce local thermal stress and cracks, refine grains, and homogenize element distribution. After cladding two layers, vibration aging treatment is performed in time to release residual stress. Reusing the failed cutter ring with remanufacturing value can save tunneling construction costs, and has good economic significance and promotion value. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a flow chart of the implementation of a method for remanufacturing a hob cutter ring by vibration-assisted laser cladding of the present invention;
[0034] Figure 2It is a distribution diagram of the cutter ring after repair in a method for remanufacturing a cutter ring of a hob by vibration-assisted laser cladding of the present invention;
[0035] Figure 3 It is a schematic diagram of a mechanical vibration-laser cladding remanufacturing system of a method for remanufacturing a hob cutter ring through vibration-assisted laser cladding of the present invention;
[0036] In the figure: 1. Vibrator; 2. Vibration isolation rubber; 3. Motor; 4. Vibration sensor; 5. Vibration transmission beam; 6. Hob cutter ring; 7. Laser head; 8. Six-degree-of-freedom robotic arm;
[0037] Figure 4 A microhardness distribution diagram of a cutter ring cross section as a function of surface depth in a method for remanufacturing a hob cutter ring by vibration-assisted laser cladding of the present invention;
[0038] Figure 5 It is a diagram of the internal grain changes of the cladding layer of a method for remanufacturing a hob cutter ring by vibration-assisted laser cladding of the present invention;
[0039] Figure 6 The present invention discloses a method for remanufacturing a hob cutter ring by vibration-assisted laser cladding, and shows changes in the surface stress of the cutter ring before and after vibration aging. DETAILED DESCRIPTION
[0040] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention is clearly and completely described below in conjunction with the accompanying drawings of the present invention. Based on the embodiments in this application, other similar embodiments obtained by ordinary technicians in this field without making creative work should all fall within the scope of protection of this application. In addition, the directional words mentioned in the following embodiments, such as "up", "down", "left", "right", "inside", "outside", etc., are only reference to the directions of the accompanying drawings. Therefore, the directional words used are used to illustrate rather than limit the invention.
[0041] The present invention provides a method for remanufacturing a hob cutter ring by vibration-assisted laser cladding, comprising the steps of:
[0042] 1) Remove the failed cutter ring from the hob, flatten it and measure its shape and size;
[0043] 2) Repair by mechanical vibration-assisted laser cladding, cladding 2 layers;
[0044] 3) Vibration aging treatment after cladding 2 layers;
[0045] 4) Repeat steps 2) and 3) until the knife circle is restored to its original size.
[0046] Specifically, the leveling process in step 1) includes:
[0047] Clean the knife ring;
[0048] Grind and clean the surface of the knife ring.
[0049] Specifically, the measurement accuracy of the shape and size in step 1) is 0.001 mm, including the inner diameter and outer diameter, width, etc. of the cutter ring, to determine the size of the cutter ring to be restored.
[0050] See also Figure 2 In step 2), gradient materials are used for laser cladding, and the cladding materials are Ni-based powder and Fe-based powder of 53μm~154μm, wherein 102 is the 1st to 4th layers, which are clad with Ni-based powder and are about 2mm thick, 103 is the 5th to 10th layers, which are clad with 80% Ni-based powder + 20% Fe-based powder and are about 2.6mm thick, 104 is the 11th to 15th layers, which are clad with 50% Ni-based powder + 50% Fe-based powder and are about 2.6mm thick, 105 is the 16th to 20th layers, which are clad with 20% Ni-based powder + 80% Fe-based powder and are about 2.6mm thick, 106 is the remaining layers, all of which are clad with Fe-based powder, and 101 is the substrate.
[0051] Nickel-based powder has good bonding properties. When used between two materials with large differences in thermal expansion coefficients, it can avoid the cladding layer from shedding and cracking due to excessive thermal stress. Since the working material is an iron-based cladding layer, the mass fraction of nickel-based powder needs to be gradually reduced from the substrate to the surface of the cladding layer until the material is completely iron-based powder, in order to reduce the excessive residual stress caused by the large difference in thermal expansion coefficients. In previous experiments, it was found that about 5 layers of cladding containing nickel-based powder are sufficient to avoid the adverse effects of residual stress between different materials.
[0052] Specifically, in step 2), the powder feeding method of laser cladding is coaxial powder feeding, the laser power range is 1400W, the scanning speed range is 10mm / s, the powder feeding amount is 10~15g / min, the overlap rate is 60%, and the laser beam is a circular spot with a diameter of 3.0mm.
[0053] Specifically, in step 2), the mechanical vibration is characterized by a one-dimensional mechanical vibration in a direction perpendicular to the laser irradiation direction, with a vibration frequency of 116.7 Hz and a vibration amplitude of 18 μm.
[0054] Specifically, in step 3), the frequency of the vibration aging treatment is any value in the sub-resonance zone of the workpiece. The frequency selected in the present invention is 60.4 Hz, which just reaches the sub-resonance, and the corresponding acceleration is 71.6 m / s 2 , the vibration aging treatment time is 30min.
[0055] See also Figure 3 The vibration table used for mechanical vibration and vibration aging is the same set. The vibration table includes: an inverted pair of 50kg / m rails connected front and back, 2 pairs of seismic isolation rubber pads, 1 vibration exciter, 1 vibration meter, 1 control box, and 1 cutter ring fixture. The vibration exciter is rigidly connected to the rail and installed at one end of the rail. The tool fixture is installed in the middle of the rail. The cutter ring, the cutter ring fixture and the rail are rigidly connected to establish a rigid connection between the cutter ring and the large mass of the rail and greatly reduce the frequency required to reach the sub-resonance zone. The vibration meter is close to the side of the cutter ring, and the seismic isolation rubber pad is placed at a position 2 / 9 of the length of the rail at both ends. This position is the node line of the rail with the minimum vibration.
[0056] Specifically, the thickness of the cladding layer formed by laser cladding is 25-30 mm.
[0057] Specifically, the residual stress measurements were performed on the heat affected zone, the surface of the 30-layer cladding layer, and the surface of the 60-layer cladding layer.
[0058] Only the preferred embodiments of the present invention are described in detail above, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention, and various changes should be included in the protection scope of the present invention.
Claims
1. A method for remanufacturing a hob cutter ring by vibration-assisted laser cladding, characterized in that: The following steps are involved: 1) Remove the failed cutter ring from the hob, flatten it and measure its shape and size; 2) The cutter ring was repaired by mechanical vibration-assisted laser cladding, with two layers of cladding. Gradient materials were used for laser cladding. The cladding materials were Ni-based powder and Fe-based powder with a diameter of 53 μm to 154 μm. Among them, the first to fourth layers are clad with Ni-based powder; From the 5th to the 10th layer, 80% Ni-based powder + 20% Fe-based powder is used for cladding; From the 11th to the 15th layer, 50% Ni-based powder + 50% Fe-based powder are used for cladding; From the 16th to the 20th layer, 20% Ni-based powder + 80% Fe-based powder is used for cladding; The remaining layers were clad with Fe-based powder; The thickness of the 1st to 4th layers is 2mm; the thickness of the 5th to 10th layers is 2.6mm; the thickness of the 11th to 15th layers is 2.6mm; the thickness of the 16th to 20th layers is 2.6mm; the total thickness of the cladding layer is 25~30mm; 3) Vibration aging treatment after cladding 2 layers; 4) Repeat steps 2) and 3) until the knife circle is restored to its original size.
2. A method for remanufacturing a hob cutter ring by vibration-assisted laser cladding as claimed in claim 1, characterized in that: The powder feeding method of laser cladding is coaxial powder feeding, the laser power range is 1400W, the scanning speed range is 10mm / s, the powder feeding amount is 10~15g / min, the overlap rate is 60%, and the laser beam is a circular spot with a diameter of 3.0mm.
3. A method for remanufacturing a hob cutter ring by vibration-assisted laser cladding as claimed in claim 1, characterized in that: The mechanical vibration is characterized by a one-dimensional mechanical vibration in a direction perpendicular to the laser irradiation direction, with a vibration frequency of 116.7 Hz and a vibration amplitude of 18 μm.
4. A method for remanufacturing a hob cutter ring by vibration-assisted laser cladding as claimed in claim 1, characterized in that: The frequency of vibration aging treatment takes any value in the sub-resonance zone of the workpiece, and the corresponding acceleration is 71.6m / s 2 , the vibration aging treatment time is 30min.
5. A method for remanufacturing a hob cutter ring by vibration-assisted laser cladding as claimed in claim 1, characterized in that Mechanical vibration and vibration aging are performed by vibrating a vibration table, which includes: An inverted pair of rails, each end of which is fixedly connected; The exciter is installed at one end of the rail and is rigidly connected to the rail; The tool fixture is installed in the middle of the rail and is rigidly connected to the rail. The tool fixture is used to rigidly clamp the tool ring; Vibration detector, used to be attached to the side of the knife ring; Two pairs of seismic isolation rubber pads are placed at a distance of 2 / 9 of the length of the rails at both ends of the rails.
6. A method for remanufacturing a hob cutter ring by vibration-assisted laser cladding as claimed in claim 1, characterized in that: In step 1), the flattening process is performed and the shape and size are measured, including: Grind the part of the surface of the used knife ring to be repaired, and then clean the surface of the knife ring; The shape and size of the waste cutter ring are measured with an accuracy of 0.001mm to determine the size of the cutter ring to be restored.
Citation Information
Patent Citations
Vibrating cladding repair technology for damaged last-stage blades of steam turbine