A low temperature resistant composite emulsion and preparation method thereof

By using organic-inorganic composite cross-linking agents and functionalized acrylic emulsions in PP artificial paper, a low-temperature-resistant composite emulsion is prepared, which solves the deformation problem of PP artificial paper under low-temperature conditions, improves its low-temperature resistance and toughness, and extends the service life.

CN117946339BActive Publication Date: 2024-10-18上海长宣化工有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410120937.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-29
Publication Date
2024-10-18
Estimated Expiration
2044-01-29

AI Technical Summary

Technical Problem

PP artificial paper is easily deformed under low temperature conditions, resulting in poor low temperature resistance. Existing toughening agents have poor dispersion in organic systems or have limited toughening effects, and cannot effectively improve the low temperature toughness of PP artificial paper.

Method used

Organic and inorganic composite cross-linking agents are used to pre-disperse natural stone powder to improve its dispersibility in organic and inorganic systems, and combined with functionalized acrylic emulsion, a low-temperature resistant composite emulsion is prepared to reduce crystallinity and enhance the properties of the composite emulsion. toughness.

Benefits of technology

It improves the low-temperature resistance of PP artificial paper, reduces curling in low-temperature environments, extends the service life, and achieves the excellent toughness and water resistance of the composite emulsion in PP artificial paper.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004686732070000071
    Figure BDA0004686732070000071
  • Figure BDA0004686732070000081
    Figure BDA0004686732070000081
Patent Text Reader

Abstract

The present invention relates to the technical field of thin film coating, and in particular to a low-temperature resistant composite emulsion and a preparation method thereof. In the method provided by the present invention, in the process of preparing the composite emulsion, natural stone powder is pre-dispersed in an acrylic ester crosslinking agent, so that the natural powder has good dispersibility in the system, can reduce the crystallinity, and has a good toughening effect on the composite emulsion, and can also greatly improve the low-temperature resistance of the prepared composite emulsion, solve the problem of uneven mixing caused by directly adding an inorganic toughening agent, and the composite emulsion finally obtained can provide excellent low-temperature resistance, flexibility and consistency, and has good application prospects in PP artificial paper.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thin film coating, and in particular to a low-temperature resistant composite emulsion and a preparation method thereof. Background Art

[0002] The preparation method of PP artificial paper includes one-step coating and two-step coating processes, wherein the one-step coating process can greatly improve production efficiency, greatly reduce energy consumption and cost, and has good application prospects. However, the one-step coating technology is still blank in China, and because the materials used for PP artificial paper are usually short-chain materials, under low temperature conditions, the crystallinity will change, which can easily cause crystal rearrangement and deformation. Moreover, under low temperature conditions, the movement of molecular chains slows down, and the internal energy between molecules decreases, resulting in greater intermolecular attraction and rearrangement of the molecular chain structure. In view of the above two combined effects, PP artificial paper materials are prone to deformation at low temperatures, resulting in poor low temperature resistance of PP artificial paper.

[0003] Chinese patent application CN 112759693 A discloses a one-component emulsion suitable for surface coating of PP artificial synthetic paper and its synthesis method. The method provides a one-component emulsion that can be coated in one step, which has the advantages of high production efficiency, low production cost, simple and easy operation, etc. In addition, the emulsion for coating PP artificial paper contains components such as acrylamide, acrylic acid, emulsifier, single soft body, hard soft body, initiator and crosslinking agent. The emulsion of this component has been proven to have good adhesion and is not easy to fall off, which can better meet the current market demand. However, the one-component emulsion for surface coating of PP artificial synthetic paper does not solve the problem of poor low temperature resistance of PP artificial paper, which will make the PP artificial paper prepared by the one-step coating process not have excellent performance at low temperatures and even lead to a short service life.

[0004] Existing studies have shown that the low-temperature toughness of PP artificial paper can be improved by adding special toughening agents and changing the structure of the coating emulsion. Among the existing toughening agents, inorganic composite toughening agents can effectively adjust the microstructure of the material, improve the interface bonding strength, and optimize the fracture mode, which can effectively improve the toughness of PP artificial paper and have good application potential. However, inorganic composite toughening agents have poor dispersibility in organic systems and are easy to absorb water, which in turn affects the performance of PP artificial paper. In addition, the toughening performance of inorganic composite toughening agents also requires high matching of the system. Although organic toughening agents have good dispersibility in organic systems, the existing organic toughening agents have limited toughening effects on PP artificial paper. Summary of the invention

[0005] In order to solve the problem that the existing PP artificial paper is not resistant to low temperature, the present invention provides a low temperature resistant and water resistant composite emulsion and a preparation method thereof. An organic-inorganic composite crosslinking agent is first prepared so that the crosslinking agent can better toughen the composite emulsion and reduce the crystallinity. The composite emulsion prepared by using the composite emulsion can provide better low temperature resistance.

[0006] The first aspect of the present invention provides a method for preparing a low-temperature resistant composite emulsion, comprising the following steps:

[0007] Step 1, taking 10-50 parts by weight of deionized water, 1-3 parts by weight of emulsifier, 20-60 parts by weight of soft monomer, 30-60 parts by weight of hard monomer, 0.5-3 parts by weight of acrylamide, 0.5-10 parts by weight of hydroxyethyl acrylate, and 0.5-3 parts by weight of functionalized acrylic emulsion, stirring and mixing to obtain an emulsion, and taking out 1-10wt% of the emulsion as a seed pre-emulsion for standby use;

[0008] Step 2, heating 30-70 parts by weight of deionized water, adding the seed pre-emulsion to mix, adding 0.03-5 parts by weight of initiator to react, then dripping the remaining emulsion to react, and adding 0.5-5 parts by weight of organic-inorganic composite crosslinking agent before the remaining emulsion is dripped, stirring, and then heat-insulating;

[0009] Step 3, after cooling, add 0.03-3 parts by weight of tert-butyl hydroperoxide dropwise, stir and mix evenly, then add 0.03-3 parts by weight of bleaching powder dropwise to react, and then keep warm;

[0010] Step 4. Finally, after cooling, add 0.2-3 parts by weight of aqueous ammonia, 0.5-5 parts by weight of adipic acid dihydrazide, 0.5-5 parts by weight of membrane aid and 0.5-5 parts by weight of alcohol ester dodecahydrate in sequence, stir and mix evenly, and obtain the low-temperature resistant composite emulsion by filtering.

[0011] Specifically, the preparation method of the organic-inorganic composite crosslinking agent in step 2 includes:

[0012] Adding an acrylic ester crosslinking agent to natural stone powder and mixing evenly to obtain an organic-inorganic composite crosslinking agent;

[0013] More specifically, the solid content of the natural stone powder after adding the acrylic ester crosslinking agent is 25-45%;

[0014] More specifically, the acrylate crosslinking agent is at least one of ethylene glycol dimethacrylate, hexanediol dimethacrylate or trimethylolpropane trimethacrylate;

[0015] More specifically, the mixing is performed by high-speed stirring at a speed of 1500 to 3000 rpm;

[0016] Natural stone powder has toughening, strengthening and stabilizing effects. In the preparation process of the above-mentioned organic-inorganic composite crosslinking agent, the natural stone powder is first pre-dispersed in the acrylic crosslinking agent, and the surface of the natural stone powder is fully impregnated with the acrylic crosslinking agent, which can reduce the water absorption of the natural stone powder during the operation process and improve the dispersibility of the natural stone powder in the organic-inorganic system;

[0017] Specifically, the functionalized acrylic emulsion in step 1 is a combination of hydroxyl acrylic emulsion and amino acrylic emulsion, and the mass ratio of the two is 0.95 to 1:1; the functionalized acrylic emulsion contains active groups (hydroxyl and amino groups), and an organic-inorganic composite crosslinking agent can be added to reduce the crystallinity, and the organic-inorganic composite crosslinking agent can be uniformly dispersed in the system and toughened in the composite emulsion, thereby improving the low temperature resistance;

[0018] Specifically, the hard monomer in step 1 is selected from one or more of styrene or methyl methacrylate;

[0019] Specifically, the soft monomer in step 1 is selected from one or more of 2-ethylhexyl acrylate and butyl acrylate soft monomers.

[0020] Specifically, the emulsifier in step 1 is a combination of a polyethylene glycol nonionic emulsifier and an alcohol ether sulfate anionic emulsifier; the mass ratio of the polyethylene glycol nonionic emulsifier to the alcohol ether sulfate anionic emulsifier is 1:2 to 2:1.

[0021] More specifically, the polyethylene glycol emulsifier includes but is not limited to fatty alcohol polyoxyethylene ether, polyethylene glycol fatty acid ester or steareth-2; the alcohol ether sulfate anionic emulsifier includes but is not limited to alcohol ether ammonium sulfate or alcohol ether sodium sulfate.

[0022] Specifically, the initiator in step 2 is selected from at least one of ammonium persulfate or potassium persulfate.

[0023] Specifically, the heating temperature in step 2 is 70-90°C.

[0024] Specifically, the reaction time of adding the initiator in step 2 is 20-40 minutes.

[0025] Specifically, the time for adding the remaining emulsion in step 2 is 2-5 hours.

[0026] Specifically, in step 2, the organic-inorganic composite crosslinking agent is added when the remaining emulsion is added to a balance of 60-1wt% of the remaining emulsion, and after adding the organic-inorganic composite crosslinking agent, the remaining emulsion is continued to be added after stirring for 1-20 minutes.

[0027] Specifically, the reaction temperature in step 2 is 78-85° C., and the insulation time is 30-120 min.

[0028] Specifically, the temperature in step 3 is lowered to 65-75°C.

[0029] Specifically, the dripping time in step 3 is 5-30min;

[0030] Specifically, the insulation time in step 3 is 5-60 minutes.

[0031] Specifically, the cooling in step 4 is to a temperature below 50° C., the stirring and mixing time is 5-30 min, and the filtration screen aperture is 200 mesh.

[0032] Specifically, the membrane auxiliary agent in step 4 is one or more of dipropylene glycol butyl ether, methyl ether or ethyl ether.

[0033] The second aspect of the present invention provides a method for preparing a low-temperature resistant composite emulsion, which comprises the following components in parts by weight:

[0034] 20-60 parts of soft monomer, 30-60 parts of hard monomer, 0.5-3 parts of acrylamide, 0.5-10 parts of hydroxyethyl acrylate, 0.5-3 parts of functionalized acrylic emulsion, 0.5-5 parts of organic-inorganic composite crosslinking agent, 0.5-5 parts of adipic acid dihydrazide, 0.5-5 parts of membrane auxiliary agent, 0.5-5 parts of alcohol ester dodecahydrate, 1-3 parts of emulsifier, 0.03-5 parts of initiator, 0.03-3 parts of tert-butyl hydroperoxide, 0.03-3 parts of bleaching powder, 0.2-3 parts of ammonia water and 40-120 parts of deionized water.

[0035] The third aspect of the present invention provides an application of the low-temperature resistant composite emulsion in the field of PP artificial paper.

[0036] The beneficial effects brought by the present invention are as follows:

[0037] 1. In the process of preparing the composite emulsion, the method provided by the present invention first pre-disperses the natural stone powder, so that the natural stone powder has good dispersibility in the system, reduces the mixing and provides a good toughening effect, and finally the composite emulsion for PP artificial paper prepared by the method can provide excellent toughness;

[0038] 2. The method provided by the present invention introduces an inorganic component - natural stone powder in the process of preparing the composite emulsion, which can reduce the crystallinity, thereby reducing the curling of the PP artificial paper prepared using the same in a low temperature environment, and improving the low temperature resistance of the PP artificial paper.

[0039] Specific embodiment

[0040] The technical solution of the present application will be clearly and completely described below in conjunction with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

[0041] The manufacturers of the functionalized acrylic emulsions described in the present invention are all Green Union (Jining) Chemical Technology Co., Ltd.; the manufacturer of natural stone powder is Chaoyang Jianyuan New Materials Technology Co., Ltd.; and the manufacturers of polyethylene glycol emulsifiers are all Tesco Chemical (Hubei) Co., Ltd.

[0042] Example 1

[0043] 1. Preparation of the organic-inorganic composite crosslinking agent described in step 2:

[0044] 10 parts by weight of ethylene glycol dimethacrylate were added to 3.5 parts by weight of natural stone powder and reacted for 2 hours to obtain an organic-inorganic composite crosslinking agent.

[0045] 2. Preparation of low temperature resistant composite emulsion:

[0046] Step 1, take 30 parts by weight of deionized water, 1 part by weight of fatty alcohol polyoxyethylene ether (AEO-3), 1 part by weight of ammonium alcohol ether sulfate (ammonium dodecyl alcohol ether sulfate), 40 parts by weight of 2-ethylhexyl acrylate, 45 parts by weight of styrene, 1.5 parts by weight of acrylamide, 5 parts by weight of hydroxyethyl acrylate, and 1.5 parts by weight of functionalized acrylic emulsion (the mass ratio of hydroxy acrylic emulsion to amino acrylic emulsion is 1:1), stir and mix to obtain an emulsion, and take out 5wt% of the emulsion as a seed pre-emulsion for standby use;

[0047] Step 2, take another 50 parts by weight of deionized water and heat it to 80°C, add the seed pre-emulsion and mix well, add 2.5 parts by weight of ammonium persulfate and react for 30 minutes, then add the remaining emulsion dropwise to react at 81°C, and when the remaining emulsion is added to a residual amount of 30wt% of the remaining emulsion, add 3 parts by weight of the above-mentioned organic-inorganic composite crosslinking agent and stir for 10 minutes, the remaining emulsion is added dropwise for 3 hours, and then kept warm for 1 hour;

[0048] Step 3, then cool down (70°C), add 1.2 parts by weight of tert-butyl hydroperoxide dropwise, stir and mix evenly, then add 1.2 parts by weight of bleaching agent dropwise to react (addition time 15 min), and then keep warm;

[0049] Step 4. Finally, after cooling to 50°C, 1.5 parts by weight of aqueous ammonia, 2.5 parts by weight of adipic acid dihydrazide, 3 parts by weight of dipropylene glycol butyl ether, and 3 parts by weight of alcohol ester are added in sequence and stirred for 20 minutes. The low-temperature-resistant and water-resistant composite emulsion on the surface of the PP artificial paper is obtained by filtration.

[0050] Example 2

[0051] 1. Preparation of the organic-inorganic composite crosslinking agent described in step 2:

[0052] 10 parts by weight of hexanediol dimethacrylate were added to 4.5 parts by weight of natural stone powder and reacted for 2 hours to obtain an organic-inorganic composite crosslinking agent.

[0053] 2. Preparation of low temperature resistant composite emulsion:

[0054] Step 1, take 10 parts by weight of deionized water, 0.6 parts by weight of polyethylene glycol fatty acid ester, 0.4 parts by weight of ammonium alcohol ether sulfate (isomeric ammonium hexadecanol ether sulfate), 30 parts by weight of 2-ethylhexyl acrylate, 30 parts by weight of styrene, 0.5 parts by weight of acrylamide, 0.5 parts by weight of hydroxyethyl acrylate, and 0.5 parts by weight of functionalized acrylic emulsion (the mass ratio of hydroxy acrylic emulsion to amino acrylic emulsion is 0.95:1), stir and mix to obtain an emulsion, and take out 1wt% of the emulsion as a seed pre-emulsion for standby use;

[0055] Step 2, taking another 30 parts by weight of deionized water and heating it to 70°C, adding the seed pre-emulsion and mixing, adding 0.03 parts by weight of potassium persulfate and reacting for 20 minutes, then dropping the remaining emulsion therein to react at 78°C, and when the remaining emulsion is added to a residual amount of 60wt% of the remaining emulsion, adding 0.5 parts by weight of the above-mentioned organic-inorganic composite crosslinking agent and stirring for 1 minute, and then keeping warm for 30 minutes;

[0056] Step 3, then cool down (75°C) and add 0.03 parts by weight of tert-butyl hydroperoxide dropwise, stir and mix evenly, then add 0.03 parts by weight of bleaching agent dropwise for reaction (dropping time 5min), the remaining emulsion is added dropwise for 2h, and then heat preservation is performed;

[0057] Step 4. Finally, after cooling (30°C), add 0.2 parts by weight of aqueous ammonia, 0.5 parts by weight of adipic acid dihydrazide, 0.5 parts by weight of methyl ether, and 0.5 parts by weight of alcohol ester dodecahydrate in sequence and stir for 5 minutes. Filter to obtain the low-temperature resistant and water-resistant composite emulsion on the surface of the PP artificial paper.

[0058] Example 3

[0059] 1. Preparation of the organic-inorganic composite crosslinking agent described in step 2:

[0060] 10 parts by weight of trimethylolpropane trimethacrylate were added to 2.5 parts by weight of natural stone powder and reacted for 3 hours to obtain an organic-inorganic composite crosslinking agent.

[0061] 2. Preparation of low temperature resistant composite emulsion:

[0062] Step 1, take 50 parts by weight of deionized water, 1 part by weight of stearyl alcohol polyether-2, 2 parts by weight of sodium alcohol ether sulfate (sodium dodecyl alcohol ether sulfate), 60 parts by weight of butyl acrylate, 60 parts by weight of methyl methacrylate, 3 parts by weight of acrylamide, 10 parts by weight of hydroxyethyl acrylate, and 3 parts by weight of functionalized acrylic emulsion (the mass ratio of hydroxy acrylic emulsion to amino acrylic emulsion is 0.98:1), stir and mix to obtain an emulsion, and take out 10wt% of the emulsion as a seed pre-emulsion for standby use;

[0063] Step 2, take another 70 parts by weight of deionized water and heat it to 90°C, add the seed pre-emulsion and mix well, add 5 parts by weight of ammonium persulfate and react for 40 minutes, then add the remaining emulsion dropwise thereto and react at 85°C, and when the remaining emulsion is added to a residual amount of 1wt% of the remaining emulsion, add 5 parts by weight of the above-mentioned organic-inorganic composite crosslinking agent and stir for 20 minutes, and then keep warm for 120 minutes;

[0064] Step 3, then cool down (65°C) and add 0.3 parts by weight of tert-butyl hydroperoxide dropwise, stir and mix evenly, then add 3 parts by weight of bleaching agent dropwise for reaction (dropping time 30min), the remaining emulsion is added dropwise for 1h, and then heat preservation is performed;

[0065] Step 4. Finally, after cooling down (10°C), 3 parts by weight of aqueous ammonia, 5 parts by weight of adipic acid dihydrazide, 5 parts by weight of ether, and 5 parts by weight of alcohol ester are added in sequence and stirred for 30 minutes. The low-temperature-resistant and water-resistant composite emulsion on the surface of the PP artificial paper is obtained by filtration.

[0066] Comparative Example 1

[0067] The difference from Example 1 is that the organic-inorganic composite cross-linking agent added in step 2 of this comparative example is replaced by natural stone powder, and the rest is the same as Example 1.

[0068] Comparative Example 2

[0069] The difference from Example 1 is that in step 2 of this comparative example, the organic-inorganic composite crosslinking agent is replaced by ethylene glycol dimethacrylate, and the rest is the same as Example 1.

[0070] Comparative Example 3

[0071] The difference from Example 1 is that the functionalized acrylic emulsion in step 2 of this comparative example is replaced by pure acrylic emulsion (manufacturer: Hefei Dibang Nanotechnology Co., Ltd.), and the rest is the same as Example 1.

[0072] Performance Testing

[0073] The composite emulsion prepared in the embodiment and the comparative example was coated on a PP film by a one-step method to obtain PP artificial paper. The performance of the PP artificial paper was tested. The test results are shown in Table 1.

[0074] Among them, the water resistance test of PP artificial paper is carried out in accordance with GB / T1034-2023; the low temperature toughness test is carried out in accordance with ASTMD638;

[0075] The low-temperature curling temperature is the temperature at which PP artificial paper curls at low temperatures. The test method is to place the PP artificial paper in a low-temperature environment for 2 hours and record the temperature at which the PP artificial paper curls.

[0076] Table 1 Performance test table of PP artificial paper prepared by composite emulsion in Examples and Comparative Examples

[0077]

[0078]

[0079] It can be seen from the above test results that the composite emulsion prepared by the method of the present invention can provide better low-temperature resistance for PP artificial paper; since the natural stone powder is directly added in Comparative Example 1, the dispersibility in the system is poor, and the water absorption of the material is increased, and the compatibility with other components is poor, it cannot be well toughened, and the final low-temperature resistance is poor; Comparative Example 2 uses a conventional acrylic cross-linking agent, which has a good compatibility with the system, but cannot well toughen the material structure, and the low-temperature resistance is poor; Comparative Example 3 uses a conventional acrylic emulsion (fewer active groups), which cannot react with the organic-inorganic composite cross-linking agent, cannot well destroy the crystallization, and has poor low-temperature resistance.

Claims

1. A method for preparing a low-temperature resistant composite emulsion, characterized in that: The following steps are involved: Step 1, taking 10-50 parts by weight of deionized water, 1-3 parts by weight of emulsifier, 20-60 parts by weight of soft monomer, 30-60 parts by weight of hard monomer, 0.5-3 parts by weight of acrylamide, 0.5-10 parts by weight of hydroxyethyl acrylate, and 0.5-3 parts by weight of functionalized acrylic emulsion, stirring and mixing to obtain an emulsion, and taking out 1-10wt% of the emulsion as a seed pre-emulsion for standby use; Step 2, heating 30-70 parts by weight of deionized water, adding the seed pre-emulsion to mix, adding 0.03-5 parts by weight of initiator to react, then dripping the remaining emulsion to react, and adding 0.5-5 parts by weight of organic-inorganic composite crosslinking agent before the remaining emulsion is dripped, stirring, and then heat-insulating; Step 3, after cooling, add 0.03-3 parts by weight of tert-butyl hydroperoxide dropwise, stir and mix evenly, then add 0.03-3 parts by weight of bleaching powder dropwise to react, and then keep warm; Step 4, finally, after cooling, add 0.2-3 parts by weight of ammonia water, 0.5-5 parts by weight of adipic acid dihydrazide, 0.5-5 parts by weight of membrane aid and 0.5-5 parts by weight of alcohol ester dodecahydrate in sequence, stir and mix evenly, and obtain the low-temperature resistant composite emulsion by filtering; The functionalized acrylic emulsion in step 1 is a combination of hydroxy acrylic emulsion and amino acrylic emulsion, and the mass ratio of the two is 0.95-1:1; The preparation method of the organic-inorganic composite crosslinking agent in step 2 comprises: Adding an acrylic ester crosslinking agent to natural stone powder and mixing evenly to obtain an organic-inorganic composite crosslinking agent; The mixing is carried out by high-speed stirring at a speed of 1500-3000 rpm; The acrylate crosslinking agent is at least one of ethylene glycol dimethacrylate, hexanediol dimethacrylate or trimethylolpropane trimethacrylate.

2. The method for preparing the low-temperature resistant composite emulsion according to claim 1, characterized in that: In step 1, the hard monomer is selected from one or more of styrene and methyl methacrylate.

3. The method for preparing the low-temperature resistant composite emulsion according to claim 1, characterized in that: The soft monomer in step 1 is selected from one or more of 2-ethylhexyl acrylate and butyl acrylate soft monomers.

4. The method for preparing the low-temperature resistant composite emulsion according to claim 1, characterized in that: The emulsifier in step 1 is a combination of a polyethylene glycol nonionic emulsifier and an alcohol ether sulfate anionic emulsifier.

5. The method for preparing the low-temperature resistant composite emulsion according to claim 1, characterized in that: The initiator in step 2 is selected from at least one of ammonium persulfate or potassium persulfate.

6. The method for preparing the low-temperature resistant composite emulsion according to claim 1, characterized in that: The heating temperature in step 2 is 70-90° C., the reaction time of adding the initiator is 20-40 minutes, and the time of dropping the remaining emulsion is 2-5 hours.

7. A low-temperature resistant composite emulsion prepared by the method according to any one of claims 1 to 6, characterized in that: By weight, it includes the following raw materials: 20-60 parts of soft monomer, 30-60 parts of hard monomer, 0.5-3 parts of acrylamide, 0.5-10 parts of hydroxyethyl acrylate, 0.5-3 parts of functionalized acrylic emulsion, 0.5-5 parts of organic-inorganic composite crosslinking agent, 0.5-5 parts of adipic acid dihydrazide, 0.5-5 parts of membrane auxiliary agent, 0.5-5 parts of alcohol ester dodecahydrate, 1-3 parts of emulsifier, 0.03-5 parts of initiator, 0.03-3 parts of tert-butyl hydroperoxide, 0.03-3 parts of bleaching powder, 0.2-3 parts of ammonia water and 40-120 parts of deionized water.

Citation Information

Patent Citations

  • Slurry containing natural stone powder as well as preparation method and application of slurry

    CN107325671A

  • Preparation method of crack-proof autoclaved aerated concrete block

    CN107459296A

  • Single-component emulsion suitable for PP artificial synthetic paper surface coating and synthesis method of single-component emulsion

    CN112759693A