A composite graphene film and preparation method thereof

By preparing a composite graphene film and utilizing the porous network structure of graphene oxide and modified graphene, the swelling problem of the graphene oxide film is solved, the interception capacity and stability of heavy metal ions are improved, and a more efficient water treatment effect is achieved. .

CN117959951BActive Publication Date: 2024-10-18CHANGSHA AVIATION VOCATIONAL & TECH COLLEGE (AIR FORCE AVIATION MAINTENANCE TECH COLLEGE) +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410226029.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-29
Publication Date
2024-10-18
Estimated Expiration
2044-02-29

AI Technical Summary

Technical Problem

The existing graphene oxide film is prone to swelling during water treatment, which affects its stability and treatment effect, resulting in insufficient interception capacity for heavy metal ions.

Method used

A composite graphene film is used, which is composed of graphene oxide and modified graphene. It is prepared by vacuum filtration and vacuum drying. The modified graphene is made by the reaction of silicon skeleton and thiourea, which increases the surface oxygen-containing functional groups and pore volume to form porous Network to improve water treatment performance.

Benefits of technology

It improves the interception capacity and stability of heavy metal ions of the composite graphene film, enhances the water treatment effect, and improves the removal rate and circulation rate of heavy metal ions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004719658040000111
    Figure BDA0004719658040000111
  • Figure BDA0004719658040000121
    Figure BDA0004719658040000121
Patent Text Reader

Abstract

The present invention relates to the technical field of graphene films, specifically a composite graphene film and a preparation method thereof, comprising the following processes: taking a graphene dispersion liquid, using a porous film as a support film, and forming a composite film on the support film by vacuum filtration; vacuum drying, removing the support film, and obtaining a composite graphene film; the graphene dispersion liquid is prepared by ultrasonically dispersing graphene oxide and modified graphene in deionized water; the modified graphene is prepared by components of graphene oxide, silicon skeleton, and thiourea. The present invention increases the flow path of water molecules by adding modified graphene prepared by graphene oxide, silicon skeleton, and thiourea to the composite graphene film components, improves the adsorption and binding of modified graphene to heavy metal ions, helps to improve the interception of heavy metal ions by the prepared composite graphene film, and improves its water treatment capacity and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of graphene films, in particular to a composite graphene film and a preparation method thereof. Background Art

[0002] With the rapid development of industrialization and the continuous growth of population, the demand for water resources is also increasing, and the resulting water shortage problem is gradually becoming prominent. In order to promote the recycling of water resources, we use membrane separation technology with low energy consumption, high efficiency and easy operation to separate and reuse heavy metal-contaminated water sources. The rich oxygen-containing functional groups on the surface of graphene oxide give it good dispersibility and film-forming properties, and it can be assembled to form a stacked structure separation membrane, showing high permeability. However, it has a strong hydration reaction with water molecules and is prone to swelling, which in turn affects the stability and treatment effect of the separation membrane in the water treatment process. Therefore, we propose a composite graphene film and a preparation method thereof. Summary of the invention

[0003] The object of the present invention is to provide a composite graphene film and a preparation method thereof to solve the problems raised in the above background technology.

[0004] In order to solve the above technical problems, the present invention provides the following technical solution: a composite graphene film is obtained by vacuum filtration of a graphene dispersion, wherein the graphene dispersion contains graphene oxide and modified graphene.

[0005] Furthermore, the mass ratio of the graphene oxide to the modified graphene is 10:(2-10).

[0006] Furthermore, the modified graphene is silicon skeleton modified graphene.

[0007] A method for preparing a composite graphene film comprises the following processes:

[0008] A graphene dispersion is taken, a porous membrane is used as a support membrane, and a composite membrane is formed on the support membrane through vacuum filtration; vacuum drying is performed, and the support membrane is removed to obtain a composite graphene film.

[0009] Furthermore, the porous membrane is made of one of polyethersulfone (PES), polyvinylidene fluoride (PVDF), and polysulfone (PSU);

[0010] The average pore size of the porous membrane is 0.20 to 0.25 μm.

[0011] Furthermore, the vacuum drying temperature is 40-60° C., and the duration is 6-12 hours.

[0012] Furthermore, the vacuum filtration is pressure-assisted, and the pressure is 0.008-0.010 MPa.

[0013] Furthermore, the porous membrane is pretreated, and the specific process is: immersed in methanol for 100 to 150 minutes, taken out, repeatedly rinsed with deionized water, and dried at 60 to 65° C. for 8 to 12 hours.

[0014] Furthermore, the graphene dispersion is prepared by ultrasonically dispersing graphene oxide and modified graphene in deionized water;

[0015] The ratio of graphene oxide, modified graphene and deionized water is 50 mg / (10-50) mg / 20 mL.

[0016] Furthermore, the modified graphene is prepared by the following process:

[0017] (1) Preparation of silicon skeleton:

[0018] Mix triethanolamine and deionized water, place at 78-83°C, and stir for 27-32 minutes; add hexadecyltrimethylammonium bromide and sodium salicylate, and continue stirring for 30 minutes;

[0019] Add ethyl orthosilicate and stir vigorously for 27 to 32 minutes; add epoxysiloxane and continue stirring for 5 to 6 hours; centrifuge, wash, and vacuum dry to obtain a reaction product;

[0020] The reaction product was placed in an acidic ethanol solution for extraction for 6 to 7 hours, and the process was repeated three times; the product was taken out and vacuum dried to obtain a silicon skeleton;

[0021] (2) Preparation of modified graphene:

[0022] Graphene oxide and silicon skeleton are mixed in distilled water, and ultrasonically treated for 60 to 75 minutes to form a dispersion; thiourea is added and ultrasonically reacted for 10 to 20 minutes; then, hydrothermally reacted at 95°C for 6 to 8 hours to form a gel; cooled to room temperature, washed with 15% ethanol, and freeze-dried to obtain modified graphene.

[0023] Furthermore, in the step (1), the ratio of triethanolamine to deionized water is 0.3 g / 100 mL;

[0024] The silicon skeleton is prepared from the following components by mass: 10 parts of ethyl orthosilicate, 0.05-0.10 parts of epoxysiloxane, 0.20-0.21 parts of triethanolamine, 1.06-1.10 parts of hexadecyltrimethylammonium bromide, and 0.23-0.25 parts of sodium salicylate;

[0025] The centrifugal speed is 4500-5000 rpm and the duration is 10 minutes.

[0026] Furthermore, in the step (1), the ratio of the reaction product to the acidic ethanol solution is 8 g / 100 mL;

[0027] The temperature of the acidic ethanol solution is 58-63°C;

[0028] In the acidic ethanol solution, the volume ratio of anhydrous ethanol to hydrochloric acid is 6:100, and the mass concentration of hydrochloric acid is 37%.

[0029] Furthermore, in the step (2), the ratio of graphene oxide to distilled water is 0.5 g / 100 mL;

[0030] The mass ratio of graphene oxide, silicon skeleton and thiourea is 10:(1-5):(25-75).

[0031] Further, the epoxysiloxane is prepared by the following process:

[0032] Mix 7-bromo-4-formaldehydebenzo[C][1,2,5]thiadiazole and anhydrous ethanol, add hydrazine hydrate, and reflux for 60 to 90 minutes; and distill under reduced pressure to obtain a bithiadiazole compound;

[0033] Add a cyclohexane solution of n-butyl lithium to tetrahydrofuran, slowly add diisopropylamine, add it all within 60 minutes, and stir for 8 to 10 hours; then slowly add N,N-dimethylformamide and trimethoxysilyl chloride, stir and react for 8 to 12 hours; distill under reduced pressure, add n-pentane, take the precipitate and dry it to obtain carbamoylsilane;

[0034] Mixing a bisthiadiazole compound and tetrahydrofuran, adding carbamoylsilane and a catalyst, stirring and reacting for 13 to 20 hours; eluting to obtain a bisthiadiazole siloxane;

[0035] Under the protection of nitrogen atmosphere, the bisthiadiazole siloxane, 1-amino-4-(2-hydroxyethyl)piperazine, potassium carbonate and potassium iodide are mixed in acetonitrile, heated to 80-90°C and reacted for 8-9h; cooled to room temperature, vacuum distilled and chromatographed to obtain hydroxysiloxane;

[0036] Under the protection of nitrogen atmosphere, a cyclohexane solution of hydroxysiloxane and n-butyl lithium is ultrasonically treated for 60 to 75 minutes, epichlorohydrin is added, and the mixture is stirred and reacted for 8 to 12 hours; the mixture is centrifuged, washed, and vacuum dried to obtain epoxysiloxane.

[0037] Furthermore, the ratio of 7-bromo-4-formaldehydebenzo[C][1,2,5]thiadiazole to anhydrous ethanol is 1 g / 100 mL;

[0038] The mass ratio of 7-bromo-4-formaldehydebenzo[C][1,2,5]thiadiazole to hydrazine hydrate is 10:(1.6-2.0).

[0039] Furthermore, the mass ratio of trimethoxysilyl chloride, N,N-dimethylformamide, n-butyl lithium and diisopropylamine is 100:(31.9-33.5):(29.2-30.0):(43.5-45.7);

[0040] The volume of the cyclohexane solution of n-butyl lithium is 50% to 60% of the volume of tetrahydrofuran;

[0041] The ratio of trimethoxysilyl chloride to tetrahydrofuran was 10 g / 100 mL.

[0042] Furthermore, the ratio of the bithiadiazole compound to tetrahydrofuran is 4 g / 100 mL;

[0043] The mass ratio of the bithiadiazole compound, carbamoylsilane and catalyst is 10:(7.0-7.2):(2.6-2.8);

[0044] The catalyst is boron trifluoride etherate (BF3·OEt2).

[0045] Furthermore, the mass ratio of the disthiadiazole siloxane, 1-amino-4-(2-hydroxyethyl)piperazine, potassium carbonate and potassium iodide is 10:(3.2-4.7):(1.9-2.8):(0.07-0.10);

[0046] The ratio of disthiadiazole siloxane to acetonitrile was 0.75 g / 100 mL.

[0047] Furthermore, the mass ratio of the hydroxysiloxane, epichlorohydrin and n-butyl lithium is 10:(1.0-1.5):(0.7-1.0).

[0048] Furthermore, the concentration of the cyclohexane solution of n-butyl lithium is 16 wt %.

[0049] Furthermore, the graphene oxide is prepared by the following process:

[0050] Mix concentrated sulfuric acid with graphite powder at 0°C and stir for 50-60 minutes; add sodium nitrate and potassium permanganate, stir and react at 3-8°C for 3 hours; raise the temperature to 35-40°C and continue stirring for 30-45 minutes; add deionized water, maintain the system temperature at 80-90°C, add hydrogen peroxide, and react until the solution turns golden yellow; centrifuge, wash with water, and dry to constant weight.

[0051] Compared with the prior art, the present invention has the following beneficial effects:

[0052] In the above technical solution, graphene is oxidized to obtain graphene oxide, whose surface contains abundant oxygen-containing functional groups, such as hydroxyl, carboxyl, epoxy, etc. These oxygen-containing functional groups can combine with heavy metal ions or form complexes through electrostatic action, thereby achieving the removal of heavy metal ions during water treatment. When graphene oxide is stacked to form a composite film, a porous network is formed, which, combined with its surface functional groups, provides nanochannels for the flow of water molecules and ion transport in water treatment, promotes the free diffusion of heavy metal ions, and increases the probability of heavy metal ions combining with oxygen-containing functional groups.

[0053] The graphene film component also contains modified graphene, which is prepared by the reaction of graphene oxide, silicon skeleton and thiourea. The silicon skeleton is obtained by hydrolyzing ethyl orthosilicate on the surface of the template hexadecyltrimethylammonium bromide to form dendritic porous silica ions with high specific surface area and pore volume. When it is combined with graphene oxide, it can increase the flow path of water molecules, improve the adsorption and binding of modified graphene to heavy metal ions, and help improve the interception of heavy metal ions by the prepared composite graphene film, and improve its water treatment capacity and stability.

[0054] In the preparation system of the silicon skeleton, epoxysiloxane is also added to functionalize the surface of the silicon skeleton and contain epoxy groups, which can increase the content of oxygen-containing functional groups on the surface of the modified graphene and improve the interception capacity of the prepared composite graphene film for heavy metal ions. The prepared silicon skeleton is mixed with graphene oxide and thiourea for reaction, and the modified graphene is prepared through the ring-opening reaction between the amino groups in the thiourea molecules and the epoxy functional groups on the surface of the silicon skeleton and graphene oxide. After freeze-drying, it is used as a gel material, which can further increase the water flow and ion transport channels in the prepared composite graphene film and improve its interception of heavy metal ions.

[0055] The epoxysiloxane is a self-made product. First, 7-bromo-4-formylbenzo[C][1,2,5]thiadiazole and hydrazine hydrate are mixed and reacted. In the reaction system, the two amino groups of the hydrazine hydrate react with the aldehyde group to form an aldimine structure to obtain a dithiadiazole compound. Then, its carbon-nitrogen double bond is reacted with carbamoylsilane to obtain a siloxane with a dithiadiazole group, which is recorded as dithiadiazole siloxane. The bromine group in its structure is reacted with 1-amino-4-(2-hydroxyethyl)piperazine, and the hydroxysiloxane obtained by the reaction is reacted with epichlorohydrin to introduce an epoxy group, thereby obtaining the epoxysiloxane described in the present application. Its molecular structure contains various structures such as benzoheterocycles and piperazine, as well as elements such as nitrogen and sulfur. It is highly selective for heavy metal ions and can cooperate with oxygen-containing functional groups such as carboxyl on the surface of graphene oxide to increase adsorption sites, coordinate and bind heavy metal ions, and promote the adsorption of heavy metal ions by the prepared composite graphene film, thereby increasing the removal rate and circulation rate of heavy metal ions, and improving its water treatment capacity and stability. DETAILED DESCRIPTION

[0056] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0057] In the following specific implementations,

[0058] The porous membrane is a polyvinylidene fluoride porous membrane with an average pore size of 0.22 μm; before use, it is immersed in methanol for 120 min, taken out, repeatedly rinsed with deionized water, and dried at 60° C. for 10 h;

[0059] Graphene oxide was prepared by the following process: 100 mL of concentrated sulfuric acid was mixed with 4.5 g of graphite powder (N / C, from Shandong Lite Nanotechnology Co., Ltd.) at 0°C and stirred for 50 min; 2.2 g of sodium nitrate and 25 g of potassium permanganate were added and stirred at 5°C for 3 h; the temperature was raised to 40°C and stirring was continued for 45 min; 200 mL of deionized water was added, the system temperature was maintained at 85°C, 5% hydrogen peroxide was added, and the solution was reacted until it turned golden yellow; centrifuged, washed with water, and dried to constant weight.

[0060] Embodiment 1: A method for preparing a composite graphene film, comprising the following process:

[0061] Step (1) preparing modified graphene:

[0062] 1.1. Preparation of epoxysiloxane:

[0063] Take 1.0 g of 7-bromo-4-formaldehyde benzo[C][1,2,5]thiadiazole and 100 mL of anhydrous ethanol, mix them, add 0.16 g of hydrazine hydrate, reflux for 60 min, and distill under reduced pressure to obtain a bithiadiazole compound;

[0064] Add 50 mL of cyclohexane solution of n-butyl lithium (2.92 g of n-butyl lithium) to 100 mL of tetrahydrofuran, slowly add 4.35 g of diisopropylamine within 60 min, and stir for 8 h; then slowly add 3.19 g of N,N-dimethylformamide and 10 g of trimethoxysilyl chloride, and stir for 8 h; distill under reduced pressure, add n-pentane, and dry the precipitate to obtain carbamoylsilane;

[0065] 4 g of a bisthiadiazole compound and 100 mL of tetrahydrofuran were mixed, carbamoylsilane and a catalyst BF3·OEt2 were added, and the mixture was stirred for 13 h; eluted to obtain a bisthiadiazole siloxane; the mass ratio of the bisthiadiazole compound, carbamoylsilane and the catalyst was 10:7.0:2.6;

[0066] Under nitrogen atmosphere, 0.75 g of distiadiazole siloxane, 1-amino-4-(2-hydroxyethyl)piperazine, potassium carbonate and potassium iodide were mixed in 100 mL of acetonitrile, heated to 80°C and reacted for 9 hours; cooled to room temperature, vacuum distilled and chromatographed to obtain hydroxysiloxane; the mass ratio of distiadiazole siloxane, 1-amino-4-(2-hydroxyethyl)piperazine, potassium carbonate and potassium iodide was 10:3.2:1.9:0.07;

[0067] Under nitrogen atmosphere protection, a cyclohexane solution of hydroxysiloxane and 16 wt% n-butyl lithium was ultrasonically treated for 60 min, epichlorohydrin was added, and the mixture was stirred for 8 h; the mixture was centrifuged, washed, and vacuum dried to obtain epoxysiloxane; the mass ratio of hydroxysiloxane, epichlorohydrin, and n-butyl lithium was 10:1.0:0.7;

[0068] 1.2. Preparation of silicon skeleton:

[0069] Take 0.3g triethanolamine and 100mL deionized water, mix them, place them at 78°C, and stir them for 32 minutes; add hexadecyltrimethylammonium bromide and sodium salicylate, and continue stirring for 30 minutes; add tetraethyl orthosilicate, and stir vigorously for 32 minutes; add epoxysiloxane, and continue stirring for 5 hours; centrifuge at 4500rpm for 10 minutes, wash, and vacuum dry to obtain a reaction product; the silicon skeleton is prepared from the following mass components: 10 parts of tetraethyl orthosilicate, 0.05 parts of epoxysiloxane, 0.20 parts of triethanolamine, 1.06 parts of hexadecyltrimethylammonium bromide, and 0.23 parts of sodium salicylate;

[0070] 8 g of the reaction product was placed in 100 mL of 58°C acidic ethanol solution (mixture of anhydrous ethanol and 37% hydrochloric acid in a volume ratio of 6:100) and extracted for 7 hours, and repeated 3 times; taken out and vacuum dried to obtain a silicon skeleton;

[0071] 1.3. Preparation of modified graphene:

[0072] 0.5 g of graphene oxide and 0.05 g of silicon skeleton were mixed in 100 mL of distilled water and subjected to ultrasonic treatment for 60 min to form a dispersion; 1.25 g of thiourea was added and subjected to ultrasonic reaction for 10 min; then, hydrothermal reaction was performed at 95° C. for 6 h to form a gel; the mixture was cooled to room temperature, washed with 15% ethanol, and freeze-dried to obtain modified graphene;

[0073] Step (2) Preparation of composite graphene film:

[0074] 50 mg of graphene oxide and 10 mg of modified graphene were added to 20 mL of deionized water and ultrasonically dispersed for 60 min to obtain a graphene dispersion. A porous membrane was used as a support membrane, and a composite membrane was formed on the support membrane by vacuum filtration with the assistance of 0.008 MPa pressure; vacuum drying was performed at 40°C for 12 h, and the support membrane was removed to obtain a composite graphene film.

[0075] Embodiment 2: A method for preparing a composite graphene film, comprising the following process:

[0076] Step (1) preparing modified graphene:

[0077] 1.1. Preparation of epoxysiloxane:

[0078] Take 1.0 g of 7-bromo-4-formaldehyde benzo[C][1,2,5]thiadiazole and 100 mL of anhydrous ethanol, mix them, add 0.18 g of hydrazine hydrate, reflux for 75 min, and distill under reduced pressure to obtain a bithiadiazole compound;

[0079] Add 55 mL of cyclohexane solution of n-butyl lithium (2.96 g of n-butyl lithium) to 100 mL of tetrahydrofuran, slowly add 4.46 g of diisopropylamine within 60 min, and stir for 9 h; then slowly add 3.27 g of N,N-dimethylformamide and 10 g of trimethoxysilyl chloride, and stir for 10 h; distill under reduced pressure, add n-pentane, and dry the precipitate to obtain carbamoylsilane;

[0080] 4 g of a bisthiadiazole compound and 100 mL of tetrahydrofuran were mixed, carbamoylsilane and a catalyst BF3·OEt2 were added, and the mixture was stirred and reacted for 16 h; eluted to obtain a bisthiadiazole siloxane; the mass ratio of the bisthiadiazole compound, carbamoylsilane and the catalyst was 10:7.1:2.7;

[0081] Under nitrogen atmosphere, 0.75 g of distiadiazole siloxane, 1-amino-4-(2-hydroxyethyl)piperazine, potassium carbonate and potassium iodide were mixed in 100 mL of acetonitrile, heated to 85°C and reacted for 8.5 h; cooled to room temperature, vacuum distilled and chromatographed to obtain hydroxysiloxane; the mass ratio of distiadiazole siloxane, 1-amino-4-(2-hydroxyethyl)piperazine, potassium carbonate and potassium iodide was 10:4.0:2.4:0.09;

[0082] Under nitrogen atmosphere protection, a cyclohexane solution of hydroxysiloxane and 16 wt% n-butyl lithium was ultrasonically treated for 68 min, epichlorohydrin was added, and the mixture was stirred for 10 h; the mixture was centrifuged, washed, and vacuum dried to obtain epoxysiloxane; the mass ratio of hydroxysiloxane, epichlorohydrin, and n-butyl lithium was 10:1.2:0.9;

[0083] 1.2. Preparation of silicon skeleton:

[0084] Take 0.3g triethanolamine and 100mL deionized water, mix them, place them at 80℃, and stir them for 30min; add hexadecyltrimethylammonium bromide and sodium salicylate, and continue stirring for 30min; add tetraethyl orthosilicate, and stir vigorously for 30min; add epoxysiloxane, and continue stirring for 5.5h; centrifuge at 4800rpm for 10min, wash, and vacuum dry to obtain a reaction product; the silicon skeleton is prepared from the following mass components: 10 parts of tetraethyl orthosilicate, 0.08 parts of epoxysiloxane, 0.20 parts of triethanolamine, 1.08 parts of hexadecyltrimethylammonium bromide, and 0.24 parts of sodium salicylate;

[0085] 8 g of the reaction product was placed in 100 mL of 60°C acidic ethanol solution (mixture of anhydrous ethanol and 37% hydrochloric acid in a volume ratio of 6:100) and extracted for 6.5 h, and repeated 3 times; taken out and vacuum dried to obtain a silicon skeleton;

[0086] 1.3. Preparation of modified graphene:

[0087] 0.5 g of graphene oxide and 0.15 g of silicon skeleton were mixed in 100 mL of distilled water and ultrasonically treated for 68 min to form a dispersion; 2.5 g of thiourea was added and ultrasonically reacted for 15 min; then hydrothermally reacted at 95 ° C for 7 h to form a gel; cooled to room temperature, washed with 15% ethanol, and freeze-dried to obtain modified graphene;

[0088] Step (2) Preparation of composite graphene film:

[0089] 50 mg of graphene oxide and 30 mg of modified graphene were added to 20 mL of deionized water and ultrasonically dispersed for 60 min to obtain a graphene dispersion. A porous membrane was used as a support membrane, and a composite membrane was formed on the support membrane by vacuum filtration with the assistance of 0.009 MPa pressure; vacuum drying was performed at 50°C for 9 h, and the support membrane was removed to obtain a composite graphene film.

[0090] Embodiment 3: A method for preparing a composite graphene film, comprising the following process:

[0091] Step (1) preparing modified graphene:

[0092] 1.1. Preparation of epoxysiloxane:

[0093] Take 1.0 g of 7-bromo-4-formaldehyde benzo[C][1,2,5]thiadiazole and 100 mL of anhydrous ethanol, mix them, add 0.20 g of hydrazine hydrate, reflux for 90 min, and distill under reduced pressure to obtain a bithiadiazole compound;

[0094] Add 60 mL of cyclohexane solution of n-butyl lithium (3.00 g of n-butyl lithium) to 100 mL of tetrahydrofuran, slowly add 4.57 g of diisopropylamine within 60 min, and stir for 10 h; then slowly add 3.35 g of N,N-dimethylformamide and 10 g of trimethoxysilyl chloride, and stir for 12 h; distill under reduced pressure, add n-pentane, and dry the precipitate to obtain carbamoylsilane;

[0095] 4 g of a bisthiadiazole compound and 100 mL of tetrahydrofuran were mixed, carbamoylsilane and a catalyst BF3·OEt2 were added, and the mixture was stirred for reaction for 20 h; eluted to obtain a bisthiadiazole siloxane; the mass ratio of the bisthiadiazole compound, carbamoylsilane and the catalyst was 10:7.2:2.8;

[0096] Under nitrogen atmosphere, 0.75 g of distiadiazole siloxane, 1-amino-4-(2-hydroxyethyl)piperazine, potassium carbonate and potassium iodide were mixed in 100 mL of acetonitrile, heated to 90°C and reacted for 8 h; cooled to room temperature, vacuum distilled and chromatographed to obtain hydroxysiloxane; the mass ratio of distiadiazole siloxane, 1-amino-4-(2-hydroxyethyl)piperazine, potassium carbonate and potassium iodide was 10:4.7:2.8:0.10;

[0097] Under nitrogen atmosphere protection, a cyclohexane solution of hydroxysiloxane and 16 wt% n-butyl lithium was ultrasonically treated for 75 min, epichlorohydrin was added, and the mixture was stirred for 12 h; the mixture was centrifuged, washed, and vacuum dried to obtain epoxysiloxane; the mass ratio of hydroxysiloxane, epichlorohydrin, and n-butyl lithium was 10:1.5:1.0;

[0098] 1.2. Preparation of silicon skeleton:

[0099] Take 0.3g triethanolamine and 100mL deionized water, mix them, place them at 83°C, and stir them for 27min; add hexadecyltrimethylammonium bromide and sodium salicylate, and continue stirring for 30min; add tetraethyl orthosilicate, and stir vigorously for 32min; add epoxysiloxane, and continue stirring for 6h; centrifuge at 5000rpm for 10min, wash, and vacuum dry to obtain a reaction product; the silicon skeleton is prepared from the following mass components: 10 parts of tetraethyl orthosilicate, 0.10 parts of epoxysiloxane, 0.21 parts of triethanolamine, 1.10 parts of hexadecyltrimethylammonium bromide, and 0.25 parts of sodium salicylate;

[0100] 8 g of the reaction product was placed in 100 mL of 63°C acidic ethanol solution (mixture of anhydrous ethanol and 37% hydrochloric acid in a volume ratio of 6:100) and extracted for 6 hours, and repeated 3 times; taken out and vacuum dried to obtain a silicon skeleton;

[0101] 1.3. Preparation of modified graphene:

[0102] 0.5 g of graphene oxide and 0.25 g of silicon skeleton were mixed in 100 mL of distilled water and ultrasonically treated for 75 min to form a dispersion; 3.75 g of thiourea was added and ultrasonically reacted for 20 min; then hydrothermally reacted at 95 ° C for 8 h to form a gel; cooled to room temperature, washed with 15% ethanol, and freeze-dried to obtain modified graphene;

[0103] Step (2) Preparation of composite graphene film:

[0104] 50 mg of graphene oxide and 50 mg of modified graphene were added to 20 mL of deionized water and ultrasonically dispersed for 60 min to obtain a graphene dispersion. A porous membrane was used as a support membrane, and a composite membrane was formed on the support membrane by vacuum filtration with the assistance of 0.010 MPa pressure; vacuum drying was performed at 60°C for 6 h, and the support membrane was removed to obtain a composite graphene film.

[0105] Comparative Example 1: A method for preparing a composite graphene film, comprising the following processes:

[0106] Step (1) preparing modified graphene:

[0107] 1.1. Preparation of modified siloxane:

[0108] Take 1.0g 2,1,3-benzothiadiazole-5-carboxaldehyde and 100mL anhydrous ethanol, mix them, add 0.11g hydrazine hydrate, reflux for 60min, and distill under reduced pressure to obtain a bithiadiazole compound;

[0109] Add 50 mL of cyclohexane solution of n-butyl lithium (2.92 g of n-butyl lithium) to 100 mL of tetrahydrofuran, slowly add 4.35 g of diisopropylamine within 60 min, and stir for 8 h; then slowly add 3.19 g of N,N-dimethylformamide and 10 g of trimethoxysilyl chloride, and stir for 8 h; distill under reduced pressure, add n-pentane, and dry the precipitate to obtain carbamoylsilane;

[0110] 4 g of the bisthiadiazole compound and 100 mL of tetrahydrofuran were mixed, carbamoylsilane and catalyst BF3·OEt2 were added, and the mixture was stirred for 13 h. The modified siloxane was obtained by elution. The mass ratio of the bisthiadiazole compound, carbamoylsilane and catalyst was 10:4.9:1.8.

[0111] 1.2. Preparation of silicon skeleton:

[0112] Take 0.3g triethanolamine and 100mL deionized water, mix them, place them at 78°C, and stir them for 32 minutes; add hexadecyltrimethylammonium bromide and sodium salicylate, and continue stirring for 30 minutes; add tetraethyl orthosilicate, and stir vigorously for 32 minutes; add modified siloxane, and continue stirring for 5 hours; centrifuge at 4500rpm for 10 minutes, wash, and vacuum dry to obtain a reaction product; the silicon skeleton is prepared from the following mass components: 10 parts of tetraethyl orthosilicate, 0.05 parts of modified siloxane, 0.20 parts of triethanolamine, 1.06 parts of hexadecyltrimethylammonium bromide, and 0.23 parts of sodium salicylate;

[0113] The subsequent process is the same as that in Example 1 to obtain a composite graphene film.

[0114] Comparative Example 2: A method for preparing a composite graphene film, comprising the following processes:

[0115] Step (1) preparing modified graphene:

[0116] 1.1. Preparation of silicon skeleton:

[0117] Take 0.3g triethanolamine and 100mL deionized water, mix them, place them at 78°C, and stir them for 32 minutes; add hexadecyltrimethylammonium bromide and sodium salicylate, and continue stirring for 30 minutes; add tetraethyl orthosilicate, and stir vigorously for 32 minutes; add γ-glycidyloxypropyltrimethoxysilane, and continue stirring for 5 hours; centrifuge at 4500rpm for 10 minutes, wash, and vacuum dry to obtain a reaction product; the silicon skeleton is prepared from the following mass components: 10 parts of tetraethyl orthosilicate, 0.05 parts of γ-glycidyloxypropyltrimethoxysilane, 0.20 parts of triethanolamine, 1.06 parts of hexadecyltrimethylammonium bromide, and 0.23 parts of sodium salicylate;

[0118] 8 g of the reaction product was placed in 100 mL of 58°C acidic ethanol solution (mixture of anhydrous ethanol and 37% hydrochloric acid in a volume ratio of 6:100) and extracted for 7 hours, and repeated 3 times; taken out and vacuum dried to obtain a silicon skeleton;

[0119] Step 1.2 is the same as step 1.3 in Example 1, and step (2) is the same as that in Example 1, to obtain a composite graphene film.

[0120] Comparative Example 3: A method for preparing a composite graphene film, comprising the following processes:

[0121] Step (1) preparing modified graphene:

[0122] 1.1. Preparation of silicon skeleton:

[0123] 0.3 g of triethanolamine and 100 mL of deionized water were mixed, placed at 78°C, and stirred for 32 min; hexadecyl trimethyl ammonium bromide and sodium salicylate were added, and stirring continued for 30 min; tetraethyl orthosilicate was added, and stirring was vigorously for 32 min; centrifuged at 4500 rpm for 10 min, washed, and vacuum dried to obtain a reaction product; the silicon skeleton was prepared from the following mass components: 10 parts of tetraethyl orthosilicate, 0.20 parts of triethanolamine, 1.06 parts of hexadecyl trimethyl ammonium bromide, and 0.23 parts of sodium salicylate;

[0124] 8 g of the reaction product was placed in 100 mL of 58°C acidic ethanol solution (mixture of anhydrous ethanol and 37% hydrochloric acid in a volume ratio of 6:100) and extracted for 7 hours, and repeated 3 times; taken out and vacuum dried to obtain a silicon skeleton;

[0125] Step 1.2 is the same as step 1.3 in Example 1, and step (2) is the same as that in Example 1, to obtain a composite graphene film.

[0126] Comparative Example 4: A method for preparing a composite graphene film, comprising the following processes:

[0127] 0.5 g of graphene oxide was mixed in 100 mL of distilled water and subjected to ultrasonic treatment for 60 min to form a dispersion; 1.25 g of thiourea was added and subjected to ultrasonic reaction for 10 min; then, hydrothermal reaction was carried out at 95° C. for 6 h to form a gel; the mixture was cooled to room temperature, washed with 15% ethanol, and freeze-dried to obtain modified graphene;

[0128] 50 mg of graphene oxide and 10 mg of modified graphene were added to 20 mL of deionized water and ultrasonically dispersed for 60 min to obtain a graphene dispersion. A porous membrane was used as a support membrane, and a composite membrane was formed on the support membrane by vacuum filtration with the assistance of 0.008 MPa pressure; vacuum drying was performed at 40°C for 12 h, and the support membrane was removed to obtain a composite graphene film.

[0129] Comparative Example 5: A method for preparing a graphene film, comprising the following process:

[0130] 60 mg of graphene oxide was added to 20 mL of deionized water and ultrasonically dispersed for 60 min to obtain a graphene dispersion. A porous membrane was used as a support membrane, and a composite membrane was formed on the support membrane by vacuum filtration with the assistance of 0.008 MPa pressure; vacuum drying was performed at 40°C for 12 h, and the support membrane was removed to obtain a graphene film.

[0131] Experiment: Take the composite graphene films obtained in Examples 1-3 and Comparative Examples 1-5 to prepare samples with a thickness of 5 μm, test their properties respectively and record the test results:

[0132] Retention capacity test: fix the sample in the filter device, place 0.1M copper chloride solution (concentration is Cf) in the stock liquid tube, use a vacuum pump to evacuate the collection bottle to form a negative pressure of 0.5MPa, collect the permeate in the collection bottle after 30 minutes, detect its concentration Cp, and calculate the retention rate of the sample after the experiment = (1-Cp / Cf) × 100%;

[0133] Cyclic stability performance test: The sample was subjected to a retention capacity test, then immersed in 0.3M hydrochloric acid for 60 minutes for desorption, taken out, washed with water, and dried; the above operation was repeated 10 times, and the retention capacity test was performed again. The changes in the initial retention rate Rp of the sample and the retention rate Rf after 10 cycles were compared, and the change rate was calculated as (1-Rf / Rp)×100%.

[0134]

[0135]

[0136] According to the data in the above table, we can clearly draw the following conclusions:

[0137] The composite graphene films obtained in Examples 1-3 are compared with the composite graphene films obtained in Comparative Examples 1-5. The test results show that:

[0138] Compared with the comparative example, the composite graphene film obtained in Examples 1-3 has higher interception rate data and lower change rate data, which fully demonstrates that the present invention improves the interception capacity and stability of the composite graphene film and has better water treatment capacity.

[0139] Compared with Example 1, in Comparative Example 1, 7-bromo-4-formaldehyde benzo[C][1,2,5]thiadiazole is replaced by 2,1,3-benzothiadiazole-5-carboxaldehyde, and the preparation process is changed to obtain modified siloxane, which is used in the preparation of silicon skeleton; in Comparative Example 2, homemade epoxysiloxane is replaced by γ-glycidyloxypropyltrimethoxysilane of equal mass; in Comparative Example 3, no siloxane is added in the preparation of silicon skeleton; in Comparative Example 4, modified graphene is obtained by reacting graphene oxide and thiourea; and the graphene film component in Comparative Example 5 is graphene oxide. Compared with Example 1, the composite graphene film obtained in Comparative Examples 1-5 has deteriorated interception rate and change rate data. It can be seen that the addition of modified graphene and the setting of its process and components in the present invention can promote the improvement of the interception capacity and stability of the composite graphene film, and help to improve its water treatment capacity.

[0140] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.

[0141] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a composite graphene film, characterized in that: Including the following processes: Taking a graphene dispersion liquid, using a porous membrane as a support membrane, and forming a composite membrane on the support membrane by vacuum filtration; vacuum drying, removing the support membrane, and obtaining a composite graphene film; The graphene dispersion is prepared by ultrasonically dispersing graphene oxide and modified graphene in deionized water; The modified graphene is prepared from components of graphene oxide, silicon skeleton and thiourea; The modified graphene is prepared by the following process: (1) Preparation of silicon skeleton: Mix triethanolamine and deionized water, place at 78-83°C, and stir for 27-32 minutes; add hexadecyltrimethylammonium bromide and sodium salicylate, and continue stirring for 30 minutes; Add ethyl orthosilicate and stir vigorously for 27 to 32 minutes; add epoxysiloxane and continue stirring for 5 to 6 hours; Centrifugation, washing, and vacuum drying are performed to obtain the reaction product; The reaction product was placed in an acidic ethanol solution for extraction for 6 to 7 hours, and the process was repeated three times; the product was taken out and vacuum dried to obtain a silicon skeleton; (2) Preparation of modified graphene: The graphene oxide and silicon skeleton are mixed in distilled water, and ultrasonically treated for 60 to 75 minutes to form a dispersion; thiourea is added and ultrasonically reacted for 10 to 20 minutes; then hydrothermally reacted at 95°C for 6 to 8 hours to form a gel; cooled to room temperature, washed with 15% ethanol, and freeze-dried to obtain modified graphene; The epoxysiloxane is prepared by the following process: Mix 7-bromo-4-formaldehydebenzo[C][1,2,5]thiadiazole and anhydrous ethanol, add hydrazine hydrate, and reflux for 60 to 90 minutes to obtain a bithiadiazole compound; Add a cyclohexane solution of n-butyl lithium to tetrahydrofuran, slowly add diisopropylamine, add it all within 60 minutes, and stir for 8 to 10 hours; then slowly add N,N-dimethylformamide and trimethoxysilyl chloride, stir and react for 8 to 12 hours to obtain carbamoylsilane; Mixing a bisthiadiazole compound and tetrahydrofuran, adding carbamoylsilane and a catalyst, stirring and reacting for 13 to 20 hours to obtain a bisthiadiazole siloxane; Under the protection of nitrogen atmosphere, bisthiadiazole siloxane, 1-amino-4-(2-hydroxyethyl)piperazine, potassium carbonate and potassium iodide are mixed in acetonitrile, heated to 80-90° C. and reacted for 8-9 hours to obtain hydroxysiloxane; Under the protection of nitrogen atmosphere, a cyclohexane solution of hydroxysiloxane and n-butyl lithium is ultrasonically treated for 60 to 75 minutes, epichlorohydrin is added, and the mixture is stirred and reacted for 8 to 12 hours to obtain epoxysiloxane.

2. The method for preparing a composite graphene film according to claim 1, characterized in that: The ratio of the graphene oxide, the modified graphene and the deionized water is 50 mg / (10-50) mg / 20 mL.

3. The method for preparing a composite graphene film according to claim 1, characterized in that: The silicon skeleton is prepared from the following components by mass: 10 parts of ethyl orthosilicate, 0.05-0.10 parts of epoxysiloxane, 0.20-0.21 parts of triethanolamine, 1.06-1.10 parts of hexadecyltrimethylammonium bromide, and 0.23-0.25 parts of sodium salicylate; The mass ratio of graphene oxide, silicon skeleton and thiourea is 10: (1-5): (25-75).

4. The method for preparing a composite graphene film according to claim 1, characterized in that: The mass ratio of 7-bromo-4-formaldehydebenzo[C][1,2,5]thiadiazole and hydrazine hydrate is 10:(1.6-2.0).

5. The method for preparing a composite graphene film according to claim 1, characterized in that: The mass ratio of the bithiadiazole compound, carbamoylsilane and the catalyst is 10:(7.0-7.2):(2.6-2.8).

6. The method for preparing a composite graphene film according to claim 1, characterized in that: The mass ratio of the disthiadiazole siloxane, 1-amino-4-(2-hydroxyethyl)piperazine, potassium carbonate and potassium iodide is 10:(3.2-4.7):(1.9-2.8):(0.07-0.10).

7. The method for preparing a composite graphene film according to claim 1, characterized in that: The mass ratio of the hydroxysiloxane, epichlorohydrin and n-butyl lithium is 10:(1.0-1.5):(0.7-1.0).

8. A composite graphene film prepared according to the preparation method according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Disiloxane ionic liquid hybridization mesoporous molecular sieve SBA-15 composite material as well as preparation method and application of composite material

    CN103706330A

  • Preparation method of nanometer titania / molybdenum disulfide composite film

    CN106179415A